kapy academy

Annealing and strengthening

14 min readUpdated Nov 2026

Anneal a part when it has to take more heat than its plastic gives straight off the printer. A controlled bake turns a PLA-HT part, which softens at around 70 °C as printed (HDT at 0.45 MPa; ordinary PLA at around 57 °C), into one that holds its shape close to 100 °C. It pays with PLA made for annealing and fiber-filled composites; on PETG, ABS, ASA or PC it only relieves stress. And every annealed part changes size: it shrinks in the plane of the layers, grows in Z and sags wherever it has no support.

Why heat changes the plastic

A printed part carries two hidden weaknesses. The first is residual stress: each bead leaves the nozzle stretched and cools quickly and unevenly, and that pull stays locked inside the part. The second is low crystallinity. PLA, the polyamides, PET and PEEK are semi-crystalline polymers, but the part cooled too fast for the chains to order themselves into crystals. A freshly printed PLA part is almost entirely amorphous.

Annealing happens inside a temperature window. Above the glass transition (Tg, about 55–60 °C for PLA) the chains can move. Below the melting point (about 150–180 °C) the part keeps its shape. While the part sits in that window, the stresses relax and the chains pack into crystals. Neither too little nor too much: right above Tg crystallization is extremely slow, it is fastest in the cold-crystallization band (about 80–110 °C for PLA), and near the melt the part slumps before it finishes.

20406080100120140160180200temperature (°C)crystallization rate~57 °C: HDT of as-printed PLA~105 °C: annealed HDT (PLA-HT)rigid, glassyTg 55–60 °Cchains move, slow crystallizationanneal here: fastest crystallizationslows down and the part slumpsmelts
PLA is annealed between the glass transition and the melt. Crystallization is fastest around 80–110 °C; just above Tg it is extremely slow, and above the band the part slumps.

What the crystals buy you is heat resistance. The crystalline regions stay rigid above Tg and hold the amorphous ones in place, so the part no longer softens at the temperature it used to. The HDT rises a long way: Polymaker's HT-PLA goes from about 70 °C as printed to about 105 °C once annealed. Stiffness and strength improve only a little. In a CNC Kitchen test on ordinary PLA, tensile strength rose 7.5 % and a hook printed lying down held 16 % more, while layer adhesion did not change. The real gain is heat; strength is a modest bonus.

The price is toughness. In unmodified PLA, the part stretches less before it breaks and handles impacts worse. The difference between the three properties is covered in Stiffness, strength and toughness.

Amorphous plastics (PETG, ABS, ASA, PC) have no crystals to grow. Heating them below their Tg only relieves stress: fewer cracks around inserts and less creep over time. Their HDT barely moves. So the result depends entirely on the filament.

Which filaments are worth the oven

Ordinary PLA

It crystallizes slowly and unpredictably. Many common grades contain enough D-lactide to stay largely amorphous; they distort a lot and gain less heat resistance than a grade made for annealing. It can work (CNC Kitchen got large temperature gains in exchange for large distortion), but treat it as an experiment, not a process.

PLA formulated for annealing

PLA-HT and grades based on resins such as Ingeo 3D870 contain nucleating agents that make them crystallize quickly and repeatably, and they reach about 100–105 °C HDT. Some grades move little when annealed: Polymaker quotes 0.3–0.6 % XY shrinkage for its HT-PLA Pro and HT-PLA-GF and publishes no figure for plain HT-PLA, so measure yours on a coupon. Look on the datasheet for an "annealed" HDT column; if there is not one, the manufacturer is not promising it. The datasheet is explained in Reading a material datasheet; the material, in PLA and its variants.

Fiber-filled engineering composites

PA-CF, PA-GF, PAHT-CF, PET-CF, PPA-CF and PPS-CF. The fiber resists distortion, and annealing finishes the crystallization the printer started. In its current documentation, the Bambu Lab wiki recommends a minimum of 80 °C for 8 h and an optimum of 120–130 °C for 5–8 h for PA-CF, PET-CF and PAHT-CF, with mechanical properties 10–20 % better; its datasheets give ranges of 80–130 °C and 6–12 h. Your spool's datasheet has the final say. These materials already start from high HDTs (PAHT-CF 194 °C, PET-CF 205 °C). Nylon also comes out of the oven dry, and its stiffness changes until it has taken up moisture again: see Nylons and polyamides. The whole family is in Carbon and glass fiber filaments.

PETG, ABS, ASA and PC

Stress relief only: as a guide, about 10–20 °C below their Tg (PETG ~60–65 °C, ABS and ASA ~80–90 °C, PC ~120–130 °C), 1–2 h and a slow cool-down. If you need heat resistance, choose a different material rather than baking: ABS and ASA, Polycarbonate and its blends.

PEEK and high-performance polymers

For these, annealing at around 200 °C is part of the normal process: without it they do not reach full crystallinity. It is often done in the printer's heated chamber or in a laboratory oven. It is covered in PPS, PEEK, PEKK and PEI.

What annealing gives you, by material (a guide; the datasheet has the final say)
Material What annealing gives you Typical schedule Dimensional risk
Ordinary PLA More heat resistance, unpredictable 70–90 °C, 30–60 min High: from several % to ~10 % in XY, Z grows, bows
PLA-HT HDT up to ~100–105 °C Per datasheet; e.g. 80–100 °C, from 30 min to several hours depending on thickness 0.3–0.6 % (Polymaker HT-PLA Pro and HT-PLA-GF); others publish no figure: measure it
PA-CF, PET-CF, PAHT-CF +10–20 % in properties, higher HDT 80 °C × 8 h, or 120–130 °C × 5–8 h Low to moderate; Bambu warns of shrinkage and warping on some geometries
PETG, ABS, ASA, PC Stress relief only, no HDT gain 10–20 °C below Tg, 1–2 h Low
PEEK Needed to crystallize ~200 °C, laboratory oven or chamber Specialist process

How to anneal

Use an oven reserved for this, never the kitchen one. Annealing releases volatile compounds, more so with fiber-filled filaments: ventilate the room and do not leave the oven unattended. A convection oven with some thermal mass inside holds a more even temperature than a static one. Domestic thermostats can overshoot by several degrees on start-up, and with PLA that difference is a slumped part. Put an independent oven thermometer next to the part and trust it, not the dial.

The schedule comes first from the filament's datasheet. Time grows with wall thickness, because the heat and the crystallization have to reach the core. For its HT-PLA-GF at 80–100 °C, Polymaker gives: under 4 mm, 30–60 min; 6 mm, 1–2 h; 8 mm, 2–4 h; 10 mm, 3–6 h. Thin parts go at the low end of the range so they do not warp.

Bury the part, clean and with the supports removed, in a granular bed that acts as a support medium: fine dry salt, fine sand or dry, unmixed plaster powder, in a metal or ceramic tray. Pack the bed down until it fills every cavity and every overhang, and cover the part with a centimeter of it. The bed holds up the softened part and spreads the heat; it reduces sagging and warping, but it does not stop shrinkage. Afterwards, the salt washes off with water.

Cutaway view of a metal tray full of fine salt inside a convection oven: a printed bracket-shaped part, with no supports, is completely buried and the salt fills its holes; beside it, an oven thermometer.
Cutaway view of a metal tray full of fine salt inside a convection oven: a printed bracket-shaped part, with no supports, is completely buried and the salt fills its holes; beside it, an oven thermometer.

Put the tray, with the part already buried, into the oven at about 60 °C, wait for the thermometer next to the part to settle, and only then raise it to the annealing temperature. That way the bed and the part heat up together, you never handle salt at 100 °C, and the inside does not lag behind. The datasheet time starts once the bed reaches that temperature.

When it is done, switch the oven off and let the part cool inside, with the door shut, to near room temperature. Taking it out hot brings back the thermal gradients the bake had removed, above all with ordinary PLA and with large parts or parts of uneven thickness.

How the dimensions change

The part does not shrink evenly: it shrinks in XY and grows in Z. During extrusion the chains are stretched along the bead; with heat they relax, and the part gets shorter along the beads and gains height between layers. In CNC Kitchen's test on ordinary PLA, a 50 mm part lost up to 10 % in XY and gained 10 % in Z. Other tests on ordinary PLA give something like 2–5 % shrinkage in XY and 0.5–2 % growth in Z. Polymaker quotes 0.3–0.6 % for its HT-PLA Pro and HT-PLA-GF, and no figure for plain HT-PLA. So the change runs from a few tenths of a percent with a grade made for annealing to several percent with ordinary PLA, and it is never the same in XY as in Z. The general physics of shrinkage is in Shrinkage and dimensional stability.

as printedXYZafter annealingshrinks along the beadsgrows between layerssags without supportdistortion exaggerated
A printed part shrinks along the beads (most in the dominant direction) and grows between layers. Whatever has no support sags.

The number depends on the print, not only on the material. Shrinkage follows the bead direction, so infill angle, wall count and orientation all change it: a solid part and one at 15 % infill, from the same file, anneal differently. A published percentage only gives you the order of magnitude.

The shape changes too. Long thin arms bow and flat plates curl. Holes go oval: a horizontal one because XY and Z move differently around it; a vertical one because X and Y do not shrink equally either when the beads run in one dominant direction. And wherever the part had no support, it sags.

Designing a part that will shrink

Do not anneal anything whose size you cannot afford to lose. Press fits, bearing seats, threads, snap fits and mating faces either stay out of the oven or are designed for it from the start.

With ordinary PLA, the distortion is not a clean factor per axis: it bows, goes oval and depends on the geometry, and scaling rarely makes up for it. With an annealing grade, you can compensate with a measure-and-correct loop:

  1. Print a coupon with long dimensions in X, Y and Z, 100 mm if it fits. On a short dimension, a reading error moves the factor a lot.
  2. Anneal it exactly as you will the real part and measure it cold.
  3. Work out a factor per axis: nominal dimension divided by measured dimension.
  4. Apply each factor to its axis, with the part oriented as it will be printed.

The general measure-and-correct method is in Iterate and measure and Dimensional calibration.

Leave material where the error will land. If a face has to come out exact, give it a 0.3–0.5 mm machining allowance and machine it after the oven: facing, drilling or reaming, never before. Heat-set inserts go in afterwards too: an insert fitted before the oven works loose during the bake (Designing for heat-set inserts).

The geometry that anneals best has walls of even thickness (thick and thin regions shrink at different rates and bend the part), generous fillets, no long unsupported overhangs and a flat base that sits fully on the bed or the tray.

Strengthening without an oven

Annealing does not fix the weak direction: layer adhesion does not change, and a part with the load running across the layers is still weak. For design, assume the part is half as strong in Z as in XY, or 30 % if the material is fiber-filled, and orient it so the main load runs along the beads (Layer adhesion and anisotropy).

Strength comes from these, biggest effect first:

  1. Orientation, with the load running along the beads: Orientation and overhangs.
  2. More walls before more infill: Walls, perimeters and infill.
  3. Ribs and fillets; bending stiffness grows with the cube of thickness: Ribs, gussets and fillets.
  4. A stronger material: Choosing a filament.
  5. The sums, before you print: Estimating whether a part will hold.

The one thing geometry cannot give a PLA part is heat resistance, and that is the only good reason to anneal. Annealed PLA-HT (HDT ~105 °C at 0.45 MPa) is semi-crystalline and its datasheet gives no HDT at 1.8 MPa: count on a service temperature of about 85 °C for light loads only, and if it will carry a serious sustained load, test it hot (Heat, cold, sunlight and chemicals). In summer, a car's dashboard in the sun reaches 70–100 °C. A loaded part there needs a fiber-filled compound: PA-CF, PET-CF or PPA-CF. Unloaded or in the shade, in the console or the glovebox, ASA, PC or annealed PLA-HT will do, and PC wherever it takes knocks. Inside a car, never PLA or PETG.

When it fails

Annealing: symptom, cause and fix
Symptom Cause Fix
The part comes out slumped or bowed The oven overshot or there was not enough bed Independent thermometer next to the part, part buried, lower temperature
No gain in heat resistance It was ordinary PLA, or the time was too short for the thickness Use an annealing grade and lengthen the time to suit the wall thickness
Cracks or blisters on the surface Trapped moisture or heating too abruptly Dry the part or the filament first (Drying and storing filament) and do not skip the hold at 60 °C
It warps as it cools You took it out hot Let it cool inside the oven with the door shut
Fits no longer go together or holes come out oval A functional face was annealed without compensation Leave a machining allowance and machine afterwards, or scale per axis from a coupon

How to test it

Anneal a coupon first (Test coupons) with the same oven, the same tray, the same bed, the same temperature and the same time you will use on the real part: change any of those conditions and the result changes. Measure it cold on all three axes and check the critical holes. If the part will work hot, load it in the oven at its service temperature before you trust it.

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.