Every wall on every layer is a closed loop, and the nozzle has to start and finish it somewhere. That mark, repeated layer after layer, forms a vertical line: the seam. You cannot get rid of it (except in spiral mode), only choose where it goes and how much it shows. On a part with corners, leave it on "Aligned" and the slicer tucks it into a corner; on a smooth, round part, paint it onto the face nobody sees or use the scarf seam; and if it has neither, give it a corner in the model.
Why the seam leaves a mark
The extruder pushes filament against a column of molten plastic that behaves like a spring. When a loop starts, the pressure has to build, and for the first few millimeters too little plastic comes out: a sunken or thin stretch. When it ends, the pressure has to drop while the nozzle slows down, and the excess bulges the end. Pressure advance cancels most of that lag, not all of it. On a calibrated machine you are usually left with a small bump at the start, from ooze during the travel and from the restart after retraction, and a tiny notch where the loop closes, from the gap the slicer leaves.

The slicer cuts the loop slightly before it gets back to the start point, so the end does not land on the opening bead and double the plastic. That margin is the seam gap. Slicer labels are quoted as they appear on screen at the end of 2026: OrcaSlicer sets "Seam gap" to 10 % of the nozzle diameter (0.04 mm with a 0.4) and PrusaSlicer sets "Seam gap distance" to 15 % (0.06 mm). Bambu Studio uses 15 % too, but only shows it in developer mode. Too small, and it leaves a bump at the seam; too large, a notch. If you adjust it, go in steps of 5 percentage points, about 0.02 mm on a 0.4 mm nozzle.
When the outer wall finishes, the extruder retracts and the nozzle moves a few tenths of a millimeter along the loop itself ("Wipe while retracting") or inwards ("Wipe on loops" in Orca, off by default). Whatever oozes then ends up on the wall or inside the part, not on the surface. Most profiles print the inner walls first, so the nozzle arrives at the start of the outer wall from inside (Walls, perimeters and infill).
Light decides where the mark shows. The eye picks up a seam through reflections: on a smooth face, flat or curved, any bump breaks the sheen; inside a corner, the geometry has already broken it.
Check the machine before you touch the slicer. A bump at the start points to too much extra restart length after retraction, to ooze during the travel, or to pressure advance set too high. A bump where the loop closes points to pressure advance set too low. A notch or a gap points to pressure advance too high or a seam gap too wide. Both machine settings are calibrated in Pressure advance and clean corners and Temperature towers and retraction tests. Strings and blobs elsewhere on the wall are a different problem: Stringing and blobs.
Where the slicer puts it
:::figure{id="seam-placement-modes" caption="The same outer wall unrolled, with one dot for each layer start. "Aligned" takes the column to the concave corner; "Nearest" makes it jump between corners; "Back" takes it to +Y; "Random" scatters it across the whole wall. Paint wins wherever the stripe reaches the wall; where it does not, the position mode takes over again."}
- topView: Top view
- front: front
- back: back (+Y)
- aligned: Aligned
- nearest: Nearest
- backMode: Back
- random: Random
- painted: Painted
- corner: concave corner
- paintedArea: painted area
- fallback: no paint: back to the mode
- layer: layer
- alongWall: along the wall
- verdictAligned: hidden in the corner
- verdictNearest: jumps around
- verdictBack: at the back, in line
- verdictRandom: zits everywhere
- verdictPainted: where you decide :::
"Aligned" exists in Orca, Bambu Studio and PrusaSlicer, and is the default in all three. It picks one point per layer so the column stays continuous, preferring concave corners first and convex ones second. On a part with corners, the seam disappears into one of them. On a cylinder it becomes a straight, visible line wherever the slicer decides.
"Nearest" starts the loop at the point closest to where the nozzle already is, while still preferring corners. It saves travel; on smooth parts the seam wanders from side to side and draws a broken diagonal. Prusa uses it in its 0.8 mm nozzle profiles, where travel time matters more than finish.
"Back", called "Rear" in PrusaSlicer, takes the column to the back of the plate (+Y). Combine it with orientation: turn the part on the plate so the face that matters least points backwards. Orca also has "Aligned back", which aligns the column and pushes it toward the back.
"Random" changes the point every layer. There is no line, but the bumps are spread over the whole wall. Travel time also goes up, and every hole or pin gets bumps at random angles, which changes its fit. Use it on organic, textured or fuzzy-skin surfaces; avoid it on smooth visible faces and on parts that have to fit.

Cura organizes it differently. "Z Seam Alignment" offers "Sharpest Corner" (the default), "User Specified", "Shortest" and "Random". With "Sharpest Corner", "Seam Corner Preference" chooses between "Hide Seam" (the default: inside corners), "Expose Seam" (outside corners), "Hide or Expose" and "Smart Hiding". With "User Specified" you give a "Z Seam Position" ("Back", "Front Left"…) or X/Y coordinates, which can be relative to each part with "Z Seam Relative".
Nothing hides the bump like a concave corner: it sits in shadow and the sheen is already broken. A convex corner leaves it in view, but the bump blends into the edge and is the easiest kind to scrape or sand off. Holes have their own loops and their own seams, and the same rules apply inside them.
Inner walls have a seam too. Orca and PrusaSlicer offer "Staggered inner seams", off by default, which offsets the start of each inner wall according to its depth so they do not stack under the outer seam. It adds strength; the look does not change.
Seam position is an object setting in the process profile: you can change it per object, but not with a modifier volume; within one part, you steer it with seam painting. That way a decorative part and a fitted part can share a plate with different seams (Modifiers by region and height).
Painting the seam
All four slicers now have a seam-painting tool (Cura since 5.11, at the end of 2025), with two brushes: one that enforces the seam ("here, yes") and one that blocks it ("never here"). It is the answer for a smooth part with a hidden face: paint a vertical stripe on the back and block the front. In Cura, painting does not work on models inside a group; you can also pin the seam by coordinates, with "User Specified" and an X/Y position.
Painting the seam sets a preference, not a fixed position. On each layer, the slicer looks for the start inside the painted area; on a layer where the stripe does not reach the outer wall, it falls back to the position mode. Paint one continuous stripe a few millimeters wide over the full height, and do not skip steps or overhangs.
The paint is stored in the project, not in the mesh. Save the project as 3MF or you will lose it, and do not count on it surviving a move from one slicer family to another (STL, 3MF or STEP for the slicer). The gesture is the same as painting colors (Assigning colors in the slicer).
The scarf seam
The name comes from the woodworker's scarf joint, and the technique reached slicers in 2024: Orca first and, within a year, Bambu Studio, Cura and PrusaSlicer 2.9. Instead of ending the loop butted against its start, the outer wall begins as a ramp: it climbs in several steps from a start height up to the full layer height. When the loop comes round, the nozzle passes over the ramp while cutting the flow. Start and end overlap along a long slope, so no single start-and-stop point is left in view.

It is off by default in all four. These are its names and default values:
| Orca | Bambu Studio | PrusaSlicer | Cura | |
|---|---|---|---|---|
| Enable | "Scarf joint seam (beta)": None / Contour / Contour and hole | "Scarf seam type", in the filament profile | "Scarf joint placement": Nowhere / Contours / Everywhere | "Scarf Seam Length" > 0 |
| Length | 20 mm | 10 mm | 20 mm | 0 (off) |
| Steps | 10 | 10 | max. segment 1 mm | "Scarf Seam Step Length" 1 mm |
| Start height | 0 | 10 % of the layer | 0 % | "Scarf Seam Start Height" 0 |
| Only on loops without corners | "Conditional scarf joint", off, 155° | "Smart scarf seam application", on, 155° | "Scarf joint only on smooth perimeters", on | — |
| Inner walls | no | yes | no | — |
In Bambu Studio the scarf lives in the filament profile, and the process can override it with "Override filament scarf seam setting".
"Conditional scarf joint", "Smart scarf seam application" and "Scarf joint only on smooth perimeters" restrict the scarf to loops without real corners. In Orca and Bambu Studio those are loops where no angle drops below 155° (adjustable), meaning no turn sharper than 25°; PrusaSlicer does not publish its threshold. A loop with a corner already hides a normal seam better. Turn that option on: it ships on in Bambu Studio and PrusaSlicer, but off in Orca. With it on, Orca also skips the scarf if the overhanging part of the wall exceeds 40 % of its width.
Before you turn on the scarf, calibrate the flow ratio and pressure advance (Flow ratio and max flow tests). Without that, the overlap leaves a faint diagonal band or a double ridge, what Prusa calls a "ghost" seam. It gets worse on overhanging walls, which is what Orca's conditional mode guards against. The scarf adds almost nothing to print time. In PrusaSlicer it does not show in the seam preview: look for it in the volumetric flow view.
Choose "Contour", not "Contour and hole", unless the holes are visible faces. A hole is a small loop: one of Ø5 mm has a perimeter of about 15.7 mm. With the 20 mm default in Orca and PrusaSlicer, the ramp covers the whole hole and then some; with Bambu Studio's 10 mm, it does not.
The seam is also a weak line
At the seam the loop is not continuous: the two ends of the bead meet end to end, with a gap of a few hundredths. Everywhere else on the wall, the continuous bead carries the hoop tension; at the seam, that tension has to cross a weld. Aligned seams form a vertical line, and that line is where tubes, heat-set insert bosses and press-fit rings split first. A boss that always cracks in the same place is cracking along its seam (Designing for heat-set inserts).
The fixes, from most to least direct: move the aligned seam to where the load is low (paint it away from the working side), turn on "Staggered inner seams" so the inner walls do not share the weak line, or add a wall (Walls, perimeters and infill). On a hidden part with no tight fits, "Random" also spreads the weakness out. The scarf overlaps the ends over a longer length, but there is no published measurement of how much strength it gains.
The seam bump stands proud by a few hundredths to a tenth of a millimeter, and in a hole or on a pin it is the high spot that decides the fit. In a fitted hole, keep the seam aligned in a zone that carries no load, or paint it there; "Random" puts a bump at every bearing angle. Print the clearance coupon with the same seam you are going to use (Real printed clearances).
Hiding the seam in the design
The slicer can only hide a seam where the part gives it room. Design that room: a vertical edge on the face nobody sees, a sharp inside corner, the junction between two shapes.
On a round part, add a small vertical feature to host the seam: a shallow V-groove, a narrow full-height flat at the back, or a rib. The slicer only treats it as a corner if the change of direction exceeds its "smooth" threshold: a few degrees of faceting will not do; a real edge of 90 to 120° will. Like the parting line on an injection-molded part, it looks intentional.
Pick the seam face when you orient the part, at the same moment you decide where the supports touch. Turn it on the plate so its back or a corner falls where "Back" puts the seam, or so the painted face is easy to reach, and keep visible faces away from the seam as you keep them away from support marks (Orientation and overhangs).
Text, logos and fine details on the outer wall add seams: each letter is a loop with a seam of its own, and with raised text on a wall the seams scatter. Place wall text so the seam can go to the corners of the letters, or move it to the top face (Minimum features and text).
Texture disguises the seam. Fuzzy skin or a modeled texture hides a random seam completely (Fuzzy skin and textures). Spiral mode has no seam, but only suits hollow parts without a lid.
Once printed, a seam on an outside corner comes off with a deburring scraper or a pass of fine sandpaper (Sanding and smoothing). If what you see on the wall is ripples or horizontal bands rather than a vertical line, it is not the seam: Wall marks: ringing, VFA and Z-banding.
When it fails
| Symptom | Cause | Fix |
|---|---|---|
| Vertical line of bumps on a smooth visible face | "Aligned" on a part with no corners | Paint it at the back, turn on the scarf, or give the seam a place in the model |
| The seam zigzags round the part | "Nearest" on a smooth part | "Aligned" or painted |
| Zits all over the wall | "Random" seam, or ooze and retraction (Stringing and blobs) | "Aligned" or painted on smooth parts |
| Bump at the start of every loop | Too much extra length after retraction, ooze on the travel, pressure advance too high | Tune retraction; check pressure advance |
| Bump where the loop closes | Pressure advance too low, seam gap too small | Calibrate pressure advance; raise the seam gap by 5 points (Orca, PrusaSlicer) |
| Notch or hole at the seam | Seam gap too large, pressure advance too high | Lower the seam gap; check pressure advance |
| Diagonal band or double ridge by the seam with the scarf on | Flow ratio or pressure advance not calibrated, scarf on an overhang | Calibrate; turn the conditional option on; limit it to "Contour" |
| The part splits along a vertical line | Aligned seams under hoop tension | Move or paint the seam, stagger the inner seams, add a wall |
| The seam ignores the painted area on some layers | The painted stripe does not cover those layers | Paint the full height |
See also
- What a slicer does: the loop, its start point and everything else the slicer decides.
- Orca, Bambu Studio, PrusaSlicer and Cura: the label table across slicers, seam included.
- Speed and cooling: outer-wall speed and its effect on the mark.
- Pressure advance and clean corners: the machine-side fix for bumps and notches.