The first layer went down perfectly, the part held for an hour, maybe three, and then one corner came a millimeter off the plate and kept rising. That is warping: the plastic shrinks as it cools and bends the part until it pulls free. PLA and PETG barely suffer it on a hot bed and a clean plate; ABS, ASA, PC and polyamide (nylon) suffer it almost every time on an open printer. Do not confuse it with a part that never stuck in the first place: the fix is different.

Why it shrinks and why it pulls at the corners

Each bead leaves the nozzle hot and shrinks as it cools toward the temperature of the air around it. But it is welded to the layer below, which is cooler and has already shrunk. The new layer ends up in tension and the ones beneath in compression, and the stack bends like a bimetallic strip. Every layer adds its share. The force bending the part grows with height, while the grip stays whatever the first layer gave it.

shrinkscompressionbedhot layerairtemperature dropliftsbond to the bedopen airshrinkscompressionbedhot layerairtemperature dropwarm chamber
Each new layer shrinks on top of one that has already cooled, and the stack curls like a bimetallic strip until the corner lifts. In a warm chamber the temperature drop is smaller and the stack stays flat.

It takes a while to show because the hot bed holds the first few millimeters flat. That base is soft, close to its glass transition, and also thin and flexible, so the stress relaxes. As the part grows and stiffens, the pull built up on the base rises until it beats the bond at its weakest point. That is why a part that looked perfect at 20 minutes lets go at two hours.

It starts at the corners because shrinkage in any direction is proportional to length, and the corner is the point furthest from the center of the footprint, half a diagonal away. The pull of two walls adds up there, and the peel starts from a point with hardly any bonded area behind it, the way tape peels from its end. A straight edge holds better because the peel has to advance along all of it at once. The usual explanation, that the corner cools first, is only part of the story: the main cause is geometric.

The force depends on three things: the material's shrinkage, the length of the base, and the temperature drop from where the plastic sets to the air around the part. The material decides the first; the design, the second; the bed and the enclosure, the third.

An example with numbers. A 150 mm ABS base, with shrinkage around 0.5–0.8 %, wants its upper layers to end up as much as 0.75–1.2 mm shorter than the layer bonded to the plate. In PLA, at 0.2–0.5 %, the difference reaches 0.3–0.75 mm at most. These are upper bounds: the base also shrinks a little and relaxes, so the real difference is smaller. But that difference is what bends the part, and it leaves a base that is not flat, wrong dimensions near the plate and, often, a nozzle that strikes the raised corner a few layers higher (Layer shifts and spaghetti).

Semi-crystalline plastics (polyamide, PP, PEEK) shrink more because, on top of thermal contraction, their chains pack into crystals as they cool: hence 1–2 % for polyamide and 1.5–2.5 % for PP. Amorphous ones (PETG, PCTG, ABS, ASA, PC) contract with temperature alone, and PLA, which is semi-crystalline, leaves the nozzle almost amorphous because it cools too fast to crystallize; anneal it and it crystallizes and shrinks a further 1–5 % in XY. Fiber-filled grades shrink far less along the bead, of the order of 0.2–0.5 %, which is why PA-CF prints well where unfilled polyamide fights you. Across the bead and in Z they shrink like their matrix: PA-CF warps less, it is not immune.

Which materials and which parts suffer

Shrinkage and warping risk by material
Material Linear shrinkage (approx.) Bed (°C) Chamber Risk on an open printer
PLA 0.2–0.5 % 35–65 (55–60) no low
PETG 0.3–0.5 % 60–80 (70) no low to medium
PCTG 0.3–0.5 % 70–80 no low to medium
ABS 0.5–0.8 % 90–110 passive (heated is better) high
ASA 0.4–0.7 % 90–110 passive high
PC 0.5–0.8 % 100–120 passive or heated very high
Unfilled polyamide 1–2 % 90–120 passive or heated very high
PA-CF / PA-GF 0.2–0.5 % along the bead 80–120 heated, recommended medium
PP 1.5–2.5 % 80–100 passive very high (and it only sticks to a PP sheet or packing tape)
TPU 0.5–1 % 30–45 no low: too soft to peel the base up

PETG does not pull like ABS. Its shrinkage is close to PLA's; when PETG warps, the cause is a large flat part, a draft or a plate it does not bond well to. ABS stands apart on two counts. It contracts a little more, and above all it sets at a much higher temperature than PETG or PLA: its 90–110 °C bed already gives that away. On an open printer, each ABS layer falls many more degrees from that point down to the air, and every degree of that drop is shrinkage pulling on the base.

PLA warping does happen, but it has specific causes: large flat parts (beyond about 150 mm), a cold room or a draft sweeping across a bedslinger, a bed below its usual 55–60 °C, a dirty plate. Fix the cause; there is no need to change material.

The shapes that warp are always the same: long, flat, thin bases; solid flat parts, at 100 % infill or with thick solid floors; parts with many solid top layers over a large area, because that skin shrinks hard and pulls; tall boxes with a long run of wall sitting on the plate. Compact, near-cubic parts or parts with a small footprint warp far less. If they are PLA or PETG and they fail, it is usually because they tip over (Brims, rafts and mouse ears); an ABS cube on an open printer can still lift its corners.

High-temperature polymers such as PEEK or PEI only print without warping in a chamber at 90 °C or more; the details are in PPS, PEEK, PEKK and PEI.

Warping or poor adhesion?

A gray ABS box half printed on a textured PEI plate: one corner and its edge have lifted a few millimeters, leaving a thin gap underneath, while the rest of the base stays flat (generated illustration)
A gray ABS box half printed on a textured PEI plate: one corner and its edge have lifted a few millimeters, leaving a thin gap underneath, while the rest of the base stays flat (generated illustration)

The signs of warping:

  • The first layer was well fused.
  • The peel starts late, at one or more corners.
  • The underside comes out curved, like a shallow dish.
  • If there was a brim, the brim lifts with the corner.
  • The layers above may show a step or marks where the nozzle struck the raised corner.

A part that never stuck is something else: the beads stay round and separate, and it shifts or comes loose early, at any point, often in one piece. The fix for that is in The first layer and bed adhesion.

These are not warping either:

  • The edge of an overhang or bridge curling upwards mid-part: that is local cooling of that edge (Overhang and bridge failures).
  • Cracks between layers higher up an ABS part: the same shrinkage stress, which breaks the weakest layer instead of lifting the base (Layers splitting apart).
  • A wide lip at the base: that is elephant's foot (The face on the bed).

Another kind of warping shows up when you remove the part: it sat flat on the plate and, once off, it bows or rocks on the table. It is the same residual stress: the plate held it in check while the part was bonded. Let it cool fully on the plate before removing it (on PEI it also releases better). The real fix lies in the chamber and the design, below. Parts that print the wrong size explains how to measure the distortion that remains.

If you recorded a timelapse, the layer where the corner starts to rise tells you how much height the bond held before giving way (Reading a failed print).

The bed and the plate: the base's grip

The bed slows warping in two ways. It keeps the lower layers soft so the stress at the edge relaxes. And it sets the strength of the bond the corner has to break. For large ABS, ASA or PC bases, use the upper half of the material's range: 100–110 °C for ABS and ASA, 110–120 °C for PC. Even so, PC sets well above anything a bed in that range delivers, so the base never gets to relax: that is why PC depends so heavily on the chamber. Do not lower the bed on these materials to make the part release sooner.

Before anything else, a clean plate and the right surface: a greasy fingerprint on one corner is exactly where the peel begins. PC and polyamide want glue on PEI; polyamide does even better on garolite or a dedicated sheet, and PP sticks only to a PP sheet or packing tape. The details for each material are in Bed prep for each material.

The edge of the plate runs cooler and catches more draft: place warp-prone parts toward the center (Many parts on one plate).

Squashing the first layer harder does not stop warping. All you get is a wider base and tighter holes in the first layers; the shrinkage does not change (The first layer and bed adhesion).

The chamber and drafts

For ABS, ASA, PC and polyamide, the enclosure helps more than anything else. It raises the air temperature around the part, so each layer cools less once it has set; it also stills the air so both sides of the part cool evenly. A passive enclosure, warmed only by the bed, sits at around 40–50 °C, depending on the machine. Machines with active chamber control reach 50–65 °C. As of late 2026, machines like the Bambu H2D, with its own heater, reach 65 °C; the Prusa CORE One has no heater but regulates the bed-warmed chamber up to 55 °C.

In practice:

  • Close the door or lid and let the chamber warm up before the first layer: 10 to 15 minutes with the bed hot. Some slicers and machines can wait for the chamber to reach a set temperature before starting.
  • Auxiliary side fan off.
  • Part cooling fan at 10–30 % for ABS, ASA and PC, raised only for overhangs and bridges. "Turn the fan off for ABS" is outdated advice.
  • Chamber and exhaust fans on low.

The layer fan for each material is in Speed and cooling.

With PLA, PVA and TPU it is the other way round: in an enclosed printer, open the door once the bed is above about 45 °C, and for PETG above about 70 °C, to avoid heat creep (Enclosures and heated chambers). For these materials, what prevents warping is a room without drafts.

Without an enclosure, a cardboard box or a tent over a bedslinger helps; keep the printer away from windows and air conditioning. The slicer's draft shield is a partial remedy that costs nothing: a single-line wall that surrounds the part and rises to its height. In PrusaSlicer it is "Draft shield" ("Disabled" / "Limited" / "Enabled"), in the skirt and brim section; in OrcaSlicer, "Draft shield" in the skirt settings; in Cura, "Enable Draft Shield" under "Experimental". It cuts sideways drafts but does not warm the air: it works for small ABS parts and does not replace an enclosure for large ones. An ordinary skirt, one or two layers tall, does nothing against warping.

ABS and ASA give off styrene, polyamide caprolactam, and all of them particles; with the door closed these build up inside, so the enclosure needs filtration or ventilation (Emissions and ventilation).

Slicer settings

Mouse ears or a brim at the corners push the peel front several millimeters out and give the corner more bond to break. On large flat parts in ABS, ASA, PC or polyamide, put ears on the corners. Brims, rafts and mouse ears covers widths, settings and how to remove them. A raft is not the remedy: the part shrinks on top of it all the same, and a large ABS raft can warp along with it.

Less solid plastic in the base helps too. On large flat parts, lowering the infill and the number of solid bottom and top layers reduces the volume that shrinks and pulls; a solid flat part at 100 % infill is the one that warps worst. If you need strength elsewhere, a height modifier keeps it where it is needed (Modifiers by region and height).

On small ABS parts, meet the minimum layer time by slowing down, not by turning up the fan. If the slicer gets there by blowing harder, warping gets worse.

Design changes

Round off the footprint corners in plan. A radius brings the corner closer to the center of the base and swaps a point-like peel front for a curved one. As a starting point from common practice, not from a standard: 5 mm or more on any base, and 10 mm or more on ABS, ASA, PC or polyamide bases longer than about 100 mm.

sharp cornersliftswarpsrounded cornersradius in planstays flat
The same base in plan. With sharp corners, the corner is a point far from the center and it lifts; with a radius in plan, the peel front is curved and the base holds.

It is a radius in plan, not a fillet on the bottom edge. That fillet removes contact area exactly where the peel begins: a 40 × 40 mm box with a 3 mm bottom fillet rests on only about 1156 of its 1600 mm². On that edge, use a 0.5 mm chamfer at 45° (The face on the bed).

Lighten large solid bases: hollow them out and stiffen them with ribs; if the function allows, add relief slots or a grid of pockets on the underside. And if another face can go down, do not stand the part on its largest flat one (Orientation and overhangs).

Split parts that are too long. A 300 mm ABS part shrinks twice as much as a 150 mm one, and two halves printed separately and joined afterwards usually warp less than the whole part (Splitting large parts).

Choose the material for the machine. On an open printer, PETG or PCTG instead of ABS when their heat resistance is enough: the heat deflection temperature (HDT) at 0.45 MPa is about 70 °C for PETG, 87 °C for ABS and 100 °C for ASA. And PA-CF instead of unfilled polyamide, bearing in mind it is abrasive: it needs a hardened nozzle, 0.6 mm as first choice and never brass, and it has to be dried before printing (Choosing a filament, ABS and ASA, Nylons and polyamides, Polycarbonate and its blends).

When it fails

Warping: symptom, cause and fix
Symptom Cause Fix
ABS, ASA or PC corners rise after an hour or more, on an open printer Large temperature drop and drafts Enclosure, door closed, preheat the chamber, mouse ears (Enclosures and heated chambers, Brims, rafts and mouse ears)
The same on an enclosed printer Auxiliary fan on or part fan high, bed low in its range, sharp corners on the footprint Auxiliary fan off, part fan at 10–30 %, bed in the upper part of its range, radius on the corners
Only one corner or one side rises Draft from that side, dirty plate at that corner, part at the edge of the plate Move the part toward the center, clean the plate, draft shield
The brim lifts with the corner The bond is weak: the plate, surface or material needs glue or garolite Bed prep for each material
A large flat PLA part lifts Cold room or draft, bed too cool, dirty plate Bed at 55–60 °C, clean plate, draft shield or a box
Polyamide or PP lifts whatever you do Wrong surface and no enclosure Garolite or a polyamide sheet, a PP sheet or packing tape, an enclosure; consider PA-CF (Nylons and polyamides, Polypropylene)
Flat on the plate, bowed once removed Residual stress Let it cool on the plate; enclosure and design changes
Cracks between layers instead of lifted corners The same stress breaks the weakest layer Layers splitting apart

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?