Sandpaper cuts the layer ridges off; a solvent melts them. Its vapor softens the outer skin of the part, surface tension pulls that skin taut and the layer lines vanish under an almost injection-molded gloss, with no dust. It works when you have a solvent that attacks your plastic and that you can handle at home: in practice, acetone with ABS or ASA, and isopropyl alcohol (IPA) with PVB. PLA and PETG have no safe household solvent, so you sand them (Sanding and smoothing).

On the left, a matt gray ABS box with visible layer lines and sharp edges; on the right, the same part after smoothing, glossy, with no layers and with its edges and relief softened (generated illustration)
On the left, a matt gray ABS box with visible layer lines and sharp edges; on the right, the same part after smoothing, glossy, with no layers and with its edges and relief softened (generated illustration)

What the solvent does

The vapor condenses on the part, which is colder than it is, and soaks into the first few tens of microns of plastic. There the polymer chains loosen: the solvent plasticizes the skin and pulls its glass transition below room temperature. That soft skin flows, and surface tension pushes the ridges into the valleys until the face is flat. The same force explains why edges round off: surface tension pulls hardest where curvature is highest, which means sharp corners and fine raised detail.

Then the solvent evaporates and the skin hardens again. It does so slowly: the part stays soft and tacky for a while and holds solvent for hours or days. As a working rule, do not touch, measure, paint or load the part until it has fully dried: give it a day.

Layer linesRounded cornerReflowed skinNarrower holeBeforeAfter
Vapor only melts the outer skin: it fills the valleys between layers, but it also rounds the corner and narrows the hole.

Some side effects work in your favor. The reflowed skin seals the gaps between the outer wall's beads, so the part ends up far less porous, more watertight and easier to clean. Others you have to plan for: corners round off, raised text and small details soften, holes narrow because their edge flows inwards, and thin walls and overhangs can sag under their own weight while they are soft. Overexposure also leaves residual stress that shows up days later as fine cracks.

Which plastic with which solvent

Which plastic with which solvent
Plastic Solvent At home? Note
ABS acetone yes the classic pair
ASA acetone yes a little slower than ABS
PVB (such as Polymaker PolySmooth or Prusament PVB) IPA ≥ 90 % yes the gentlest route
HIPS d-limonene no can soften it, but there is no proven procedure
PLA ethyl acetate (partial); DCM, THF no sand and prime
PETG / PCTG DCM no sand
PC DCM no sand
PA, TPU, PP none practical no sand; industry smooths sintered PA
Resin none no sand and prime after washing and curing

Fiber-filled ABS and ASA and blends such as PC-ABS smooth unevenly: you get matt patches or exposed fiber. Try an offcut first.

The trouble with PLA is that acetone does nothing to it, and the solvents that do attack it sit on the far side of the line between workshop and laboratory. Dichloromethane (DCM) is classed by IARC as Group 2A, probably carcinogenic, and it goes straight through nitrile gloves. Tetrahydrofuran (THF) is highly flammable and forms explosive peroxides in storage. Ethyl acetate is the least bad option, but its effect is partial and depends on the formulation: matt, silk and filled PLAs react unpredictably. For PLA, sand and prime. Resin is finished the same way, after Washing and curing resin parts.

PVB exists precisely because of this. It is a filament that prints like PLA (nozzle around 215 °C, bed at 60–75 °C, no enclosure) and it is sold because IPA dissolves it. IPA is much less aggressive than acetone and a good deal less volatile: at room temperature it evaporates about five times more slowly, which is why its vapor works more slowly. The catch: PVB has little heat resistance, much like PLA, and needs drying at 45–55 °C for 6–8 h. The material itself is covered in Functional specialty filaments.

For smoothing, ABS and ASA are interchangeable: acetone works on both. If the part lives outdoors, pick ASA because it stands up better to UV; ABS and ASA explains why.

Cold acetone with ABS and ASA

You need a container with a lid that closes but does not seal under pressure. A glass jar is best, because you can watch the part without opening it; a metal tin also works. Avoid containers made of PS, ABS, PC or acrylic, which acetone attacks; PP and PE hold up, but many food tubs do not say what they are made of. Line the inside walls with kitchen roll soaked in acetone, without leaving a puddle in the bottom. Stand the part on something that will not react (a piece of glass, metal or folded aluminum foil) so it touches nothing wet, and close the lid.

LidSoaked kitchen rollStandClosed, not sealedAcetone vaporDenser at the bottomSmooths firstNo flames, heaters or sparks
Soaked paper on the walls and the part raised: vapor reaches it from every side, but it pools at the bottom and the base smooths first.

You do not need heat. Acetone boils at 56 °C, and at room temperature it evaporates fast enough to saturate the container in minutes. The paper gives a large evaporating surface on every side, so the vapor reaches the part evenly instead of rising from a puddle. Pure vapor weighs about twice as much as air; the saturated mix is only a little heavier than air, enough for the bottom of the container to be richer. That is why the base of the part gets overexposed first. Turn it between passes or raise it above the densest layer.

It takes anywhere from tens of minutes to a couple of hours, depending on temperature and on the size of the container and the part. There is no fixed figure: check every 15–20 minutes and stop as soon as the lines disappear. The end point is a gloss that still looks wet. Waiting longer only rounds and sags.

Polymaker documents a hot method: the closed container on a heated bed or hotplate at 65–75 °C, in passes of 1–3 minutes. It is faster, but it heats the acetone above its boiling point, fills the container with slightly pressurized vapor and lets it escape through the lid right above a hot surface, next to the printer's relay, power supply and fans. Do not do it at home. Cold is slower, but you are not heating a flammable solvent.

Brushing on liquid acetone or dipping the part in it is fine for local touch-ups and for gluing, but it dissolves unevenly, leaves runs and eats into thin walls quickly. Vapor is more even.

When you finish, lift the part out by its stand, not by a face: the skin is soft and will keep your fingerprints. Leave it to dry somewhere ventilated for at least 30 minutes before touching it, and a day before measuring, painting or loading it. Cap the bottle and let the paper dry outdoors before throwing it away.

IPA with PVB

Use IPA at 90 % or more. 70 % also works, but it takes longer and the leftover water can cloud the surface. The chemistry is the same; what changes is how you apply it:

  • Closed container with IPA vapor: the set-up from the previous section, with alcohol instead of acetone.
  • Spray or brush for specific areas and touch-ups: leave it to dry for at least 30 minutes and repeat if needed. On large faces spraying comes out uneven, so give several light coats rather than one soaking one.
  • Ultrasonic mist station: Polymaker's Polysher, now discontinued, was the reference and took about 30–60 minutes per part. If you get hold of one, the part has to fit in the chamber.

Do not heat IPA above about 40 °C, the limit Polymaker gives. Add the solvent's softening to PVB's low heat resistance and the part sags; the 60 °C bed some workarounds suggest is well past that limit.

Plenty of people buy PVB for its transparent version. What turns a clear filament milky is the light scattered by the layer lines, and smoothing erases the outer ones. The joints between beads inside still scatter some light, so a thick part comes out translucent and fairly clear, not like glass. Print it solid (100 % infill, or a single wall in vase mode), slowly and a little hotter; the thinner and more solid the wall, the closer it gets to transparent.

The trade-off: Polymaker warns that IPA smoothing reduces PVB's mechanical and thermal strength and advises against it on functional parts. Whatever the part is for, let it dry thoroughly: a thin part that holds alcohol goes soft.

Safety

The main risk is fire, and the numbers explain the rules. Acetone has a flash point of about −20 °C and a lower explosive limit of around 2.5 % in air. IPA's flash point is about 12 °C and its lower limit is around 2 %. In other words: at room temperature both give off enough vapor to burn, acetone even below freezing. And escaping acetone vapor, heavier than air, spreads along the floor to a boiler pilot light, a heater, a light switch or your own printer's hot bed.

As for health, acetone and IPA are irritants at high concentrations (headache, dizziness), but at a hobbyist's level of exposure they have no known chronic effects. Gloves matter more than they seem to: acetone gets through disposable nitrile in one to three minutes. The genuinely dangerous ones are DCM and THF, and they have no place in a home workshop; methyl ethyl ketone (MEK) is more aggressive and more toxic than acetone, and not worth it at home either. There are closed stations for the stronger solvents, such as Zortrax's Apoller, which runs on acetone or MEK, precisely so the vapor never reaches the room. How to ventilate the room is covered in Emissions and ventilation.

Keep solvents in their original containers, closed and away from heat. Let used paper and spent IPA evaporate outdoors or take them to a recycling center; never pour them down the drain in quantity. IPA from washing resin is a different case: it is contaminated and handled as Handling resin safely explains.

How much the dimensions change

Smoothing always changes dimensions and rounds edges: mask the faces that have to fit. The skin material moves; it does not disappear. Flat faces barely change, but edges round off, relief and engraving soften and holes narrow. On a smoothed bar, length tends to drop slightly and width and thickness to grow a little. The change is not a uniform offset you can compensate for in the model with a single figure.

A typical cold pass changes dimensions by one to a few tenths of a millimeter, depending on time and geometry. One manufacturer quotes 0.1–0.3 mm, but take that as a guide and measure your own case. Details smaller than about 1 mm lose definition.

The rule is to measure a coupon smoothed with your exact set-up and time, and design afterwards. It is the same loop as in Iterate and measure. For the fits themselves, see Choosing the fit: clearance, transition, interference and Real printed clearances.

As for strength, a well-judged treatment keeps the tensile strength of ABS the same or raises it a little, because the sealed skin has fewer notches. But overexposure makes the part brittle, and for PVB Polymaker documents a loss of strength and heat resistance. Do not count on gaining anything: treat smoothing as a cosmetic process.

Designing and masking for smoothing

Decide which faces get smoothed. A display housing can shine all over; a functional part keeps its press fits, threads, snap-fits and bearing seats crisp. Vapor reaches every exposed surface, so protect whatever has to stay on size: plug holes with a bolt or a rod of the nominal size and cover faces with aluminum tape or a thin film of petroleum jelly. The other way out is to split the part in two, smooth only one half and join them afterwards; acetone itself welds ABS, as Gluing and welding printed parts describes.

In the model:

  • Increase the clearance where a smoothed face mates with another. Start from the usual figure for your machine class (0.20 mm per side on a modern bedslinger, 0.15 mm on an enclosed CoreXY) and add the change you measured on your coupon.
  • Put a fillet or a chamfer wherever you want a soft edge with a controlled radius, instead of whatever the vapor leaves.
  • Avoid unsupported walls thinner than 1 mm: they sag while soft.
  • Give raised text a heavier stroke and make it at least 0.6–1 mm tall.

In the slicer, add more walls (3 or more) so the solvent cannot reach the gaps in the infill. A lower layer height leaves shallower valleys, and a shorter pass levels them.

Smoothing gives gloss and seals the surface, but it adds no color and no hard protective layer. If you are going to paint the part (Painting and priming), let it dry fully before priming.

When it fails

Smoothing: symptom, cause and fix
Symptom Cause Fix
The base is overexposed and the top still shows layers The vapor has stratified Turn the part between passes or raise it higher
The part is soft, sagging and the text has gone Too long or too hot Shorter passes; check sooner
A white or cloudy haze Moisture condensed on the part (a cold, damp room) or residue on the surface Dry the part and smooth somewhere dry; with IPA, raise the concentration
Fine cracks days later Overexposure Smooth less
A hole no longer takes its screw Its edge has flowed inwards Plug it next time, or open it up in the model by what you measured on the coupon
The support marks are still there, now glossy Vapor does not remove scars or burrs Clean them off first (Support removal and cleanup)

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?