kapy academy

Stiffness, strength and toughness

14 min readUpdated Nov 2026

Three words get used as if they were one, and a material can be good at one and poor at another. You print a sensor bracket in PLA. On the bench it holds the sensor without moving a tenth of a millimeter. It falls on the floor and breaks into three pieces. The PETG copy gives a little more when you push it, but it survives the drop. Same shape, opposite failures, and people call both of them "strong". Each has its own number on the datasheet, and which one rules depends on how your part can fail.

Three different questions

Stiffness tells you how much a material deforms under a small load, one that still lets it spring back when you remove it. On the datasheet it appears as an elastic modulus: Young's modulus (from a tensile test) or flexural modulus (from a bending test), both in GPa. For a part loaded in bending, use the flexural one; the tensile figure on filament datasheets often does not add up, and ABS, for example, gives 3.8 GPa in tension and 1.9 in flexure. Stiffness measures how much a part gives, not when it breaks.

Strength is the stress at which the material stops recovering (the yield strength) or breaks (the tensile strength), in MPa. In a brittle material the two coincide: it breaks where it stops being elastic. A ductile one reaches yield first, and the part stays permanently bent before it breaks. For design, yield is usually the limit that counts: a hook that has opened up has already failed, even if it is still in one piece.

Toughness is the energy a material absorbs before it breaks. Filament datasheets do not give it a number of its own: you infer it from elongation at break (%) and notched Charpy impact strength (kJ/m²).

Hardness is a fourth property, separate from all three. It measures how well the surface resists scratching or denting. A hard material can be brittle. The Shore scale, the one used for TPU, is covered in TPU and flexible filaments.

All three on one curve

Pull on a test bar and plot stress (force per unit area) against strain (elongation per unit length). The three properties are three readings of that curve.

strainstresselastomer (TPU)ductile (PETG, PC, nylon)brittle (PLA, fiber-filled)slope = stiffnessyield pointpeak = strengtharea = toughness
All three properties are read off the same curve: the slope of the straight section is stiffness, the peak is strength and the area up to fracture is toughness. The brittle material's curve climbs more steeply and stops early; the ductile one yields at the knee and keeps absorbing energy.

The slope of the initial straight section is stiffness. The highest point is strength. The area under the whole curve, up to fracture, is toughness. It is an area because energy is force times distance: if one axis is force per unit area and the other is elongation per length, the area under the curve is energy per unit volume.

There are three typical shapes. The brittle one climbs steeply and stops abruptly near the peak, with almost no plastic deformation, so it encloses little area; that is PLA and the fiber-filled grades. The ductile one is less steep, yields at a knee and then keeps stretching before it breaks, enclosing a large area: that is how PETG, PC and nylon behave. The elastomer's is almost flat, stretches enormously and recovers its shape. That is TPU: an 85A has a Young's modulus of about 0.01 GPa, more than two orders of magnitude below PLA.

These are bulk-polymer curves. In a printed test bar the order can even reverse: PLA stretches further than PETG in a slow test. Further down you will see why that number misleads.

This curve explains the bracket from the opening. PLA's line is steeper (a flexural modulus of 2.8 GPa against 1.8 on Bambu's datasheets), so it deflects less: under the same load, the part moves less. PETG yields at the knee and keeps absorbing energy: that is why it survives the impact.

What separates the common filaments least is strength. On Bambu's datasheets, tensile strength along the bead is 35 MPa for PLA Basic, 51 for PETG Basic, 52 for ASA and 62 for PC. PLA is not "stronger" than PETG; on those sheets it is the weakest. Stiffness and, above all, toughness separate them far more. And in a real part, printing it so the load crosses the layers costs you half the strength, as much as or more than you gain by moving from one common family to another.

Part stiffness: material and geometry

What you feel when you push is the stiffness of the part, not of the material. In a plate or beam working in bending, deflection is proportional to 1 / (E · t³), where E is the modulus and t the thickness. The modulus counts once. Thickness counts cubed.

relative deflection, same loadPETG 3 mm · 1.00PLA 3 mm · 0.64PETG 3.5 mm · 0.63PETG 4 mm · 0.42PAHT-CF 3 mm (dry) · 0.42deflection proportional to 1 / (E · t³)
Same load on the tip of a cantilever. Half a millimeter more PETG gives the same deflection as switching to PLA, and one more millimeter matches a dry carbon-fiber nylon, without giving up PETG's toughness.

Take a 3 mm PETG cantilever as the reference (deflection 1.00), with the book's design moduli, a little below the datasheet values to cover what a real part has and a test bar does not: PETG 1.6 GPa, PLA 2.5 and dry PAHT-CF 3.8 along the bead. The same in PLA: 1.6 / 2.5 = 0.64. In 3.5 mm PETG: (3 / 3.5)³ = 0.63. In 4 mm PETG: (3 / 4)³ = 0.42. In 3 mm PAHT-CF: 1.6 / 3.8 = 0.42. A fiber-filled nylon loses part of that modulus once it takes up moisture from the air, so the real comparison is even less favorable to it.

The rule: if a part is too floppy, try geometry first (more thickness, a rib, a deeper section) and material second. Add material where the bending moment is highest, usually at the root, not across the whole part. Ribs, gussets and fillets works through the cube law and how much stiffness each gram of rib buys.

Stiffness also depends on direction. PAHT-CF's flexural modulus is 4.2 GPa along the bead and 1.8 between layers: fiber only stiffens in the direction the nozzle laid it down.

And it depends on temperature. Datasheet values are measured at about 23 °C; as you approach the glass transition temperature the modulus collapses, and a PLA bracket that is rigid in the workshop sags inside a car in the sun. Under load, an amorphous plastic works up to 15–20 °C below its HDT at 0.45 MPa: PLA about 40 °C, PETG 50, ASA 80–85. A semi-crystalline one, such as nylon, is judged by its HDT at 1.8 MPa (Heat, cold, sunlight and chemicals).

Sometimes the stiffness has to come from the material: precision jigs, sensor and camera mounts, long thin arms with no room for more thickness. That is what fiber-filled composites are for; compared with the same maker's unfilled version they gain of the order of 40 % in stiffness or more (PLA 2.8 → PLA-CF 3.9 GPa on Bambu's datasheets). Carbon and glass fiber filaments covers them.

A part is only as strong as its weak spot

The datasheet strength comes from a clean test bar pulled along the bead. A printed part breaks at its weakest point, and two things matter more than the choice of material.

The first is the layers. Across the layers a part is weaker and breaks without warning: design with Z at 50 % of XY unfilled and 30 % fiber-filled, and orient the part so the main load runs along the beads (Layer adhesion and anisotropy).

The second is stress concentrators. A sharp inside corner, a notch, a hole or a slot multiplies the local stress: at a sharp corner it can double or triple. A pronounced layer line on a curved surface behaves like a row of small notches. A generous fillet at the root of a bracket is usually worth more than a stronger filament; how to model it so it prints well is in Ribs, gussets and fillets.

A load held for weeks, or repeated thousands of times, breaks a part below the datasheet value, which comes from a short test: that is the subject of Creep and fatigue. To work out whether a given part will take a given load, follow Estimating whether a part will hold.

Toughness does not fit in one number

You can read stiffness off the datasheet; toughness you cannot. It depends on how fast the load arrives, whether there is a notch, the temperature and, in a printed part, the bond between layers. A slow tensile test and a fast notched impact measure different things.

The datasheets show it. On Bambu's, PLA Basic stretches 12 % before breaking along the bead, more than PETG Basic's 9.5 %. In notched Charpy on a printed bar, PC gives 7.5 kJ/m², level with PLA (7.9) and far below PETG (21.6) and ABS (21.5). Yet a PC part that gets dropped survives where a PLA one shatters.

Elongation misleads because the test is slow. Pull slowly and PLA has time to stretch; under an impact it does not, and it cracks. Charpy misleads because it uses a notch. PC is notch-sensitive: a sharp notch (the test's, or a pronounced layer line) concentrates stress at a point where the material never gets to yield. Without notches and with fillets, PC is very tough. So do not read the 3.8 % elongation of its printed bar as proof that it is brittle either.

In practice, use the qualitative scale in Filament comparison table: PLA brittle, PETG medium-high, PC very high, nylon very high, TPU does not break, fiber-filled brittle to medium. Then check it: drop and bend a test coupon, or the part itself, printed in its final orientation. Test coupons explains how to do it with little plastic.

Between layers, toughness falls faster than strength. PLA's elongation goes from 12 % in XY to 7.5 % in Z; PETG's from 9.5 % to 5.2 %. That is why a Z fracture is clean and sudden even in a tough material.

In anything that bends on purpose, such as a clip or a tab, toughness shows up as allowable strain. For a one-off assembly: 2 % in PLA, 3–4 % in PETG and PC, 6 % in conditioned nylon, 8–10 % in PP; less with repeated use. The formula and sizing are in Print-friendly snap fits.

This is how to read a broken part. A brittle one snaps cleanly, with a glassy face and no warning. A tough one bends, stress-whitens and stretches before it lets go: it has absorbed far more energy.

What toughness depends on

Fiber

It adds stiffness at the cost of elongation and toughness: every fiber end is a place where a crack can start. On Bambu's V2.0 datasheets, PLA goes from 12.2 % elongation to 8.4 % in PLA-CF; PET-CF stays at 4.1–4.5 % and PPA-CF at 3.2 %. The exception is PETG-CF, which keeps almost all of its base's ductility (11.2 to 10.4 %). Even so, a clip or a part that will be dropped calls for the unfilled base.

Cosmetic additives

Silk PLA stretches 3.5 % in XY and 1.7 % in Z: use it as a finish, never for a working part. The mineral filler in matt PLA also weakens layer bonding. The details are in PLA and its variants.

Impact-modified grades

Grades such as Bambu's PLA Tough+ multiply notched impact strength (72.3 against 7.9 kJ/m²) at the cost of 30 % less modulus and lower strength between layers. PCTG takes knocks better than PETG with similar stiffness. They are the logical step up from PLA when a part gets knocked about but does not get hot. PETG, PCTG and other copolyesters compares them.

Water, in nylon

Freshly printed and dry, nylon is stiff and fairly brittle; conditioned (in equilibrium with the moisture in the air), it is much tougher and much less stiff. On Polymaker's PolyMide CoPA datasheet, going from dry to wet (immersion, the extreme case), the modulus falls from 2.70 to 0.72 GPa and notched Charpy rises from 6.9 to 27.7 kJ/m². A nylon clip that snaps on day one may work a few weeks later. So do not lump nylon and PETG together as "tough": nylon's toughness depends on how much water it holds. Nylons and polyamides explains it.

Cold

PLA handles it worst; ABS and ASA hold their toughness better. Unnotched PC stays tough below zero, but with notches and thick walls it turns brittle sooner. PC-PBT is sold for sub-zero use: its maker says it keeps a good share of its impact strength at −30 °C. More in Polycarbonate and its blends and Heat, cold, sunlight and chemicals.

Choosing by how the part can fail

Start from what the part has to do; the property that matters follows from that.

Which property matters for what the part does
What the part must do Property that matters What to read on the datasheet First choices (unfilled → fiber-filled)
Hold a sensor, camera or jig perfectly still Stiffness Flexural modulus, in XY and Z PLA; if you cannot add thickness, PLA-CF (3.9 GPa), PAHT-CF (4.2 dry) or PET-CF (5.3)
Carry a static load Strength along the bead, and creep Tensile strength in XY and Z (and yield strength if the sheet gives it) Orientation first; PLA at room temperature; PETG, ASA or PC if there is heat
Survive drops, knocks or squeezing Toughness Qualitative scale, elongation, drop test on a coupon PETG, PCTG, PC or nylon
Bend on purpose (snap fit, clip, latch) Allowable strain Allowable strain table PETG, PC, nylon, PP; never silk or fiber-filled PLA
Absorb impacts, grip, seal Elasticity (elastomer) Shore hardness TPU

The full method, from the failure you fear to the material family, is in Choosing a filament.

When it fails

Symptom, cause and fix
Symptom Cause Fix
The PLA part shatters when dropped or squeezed Stiff and brittle: it does not give under a fast load Switch to PETG, PCTG or PC and fillet the corners
The PETG bracket flexes under a light load Low modulus (1.8 GPa against PLA's 2.8) Thicken the section or add a rib before changing material: thickness counts cubed
The carbon-fiber clip breaks on first use Fiber reduces elongation Use the same material without fiber
The nylon clip snaps on day one Dry nylon is at its most brittle Let it condition before testing it and design with conditioned values
The part breaks at a sharp inside corner well below the expected load Stress concentrator Fillet the root
The part splits cleanly along a layer Low strength and toughness in Z Reorient the part; the printing causes are in Layers splitting apart
The hook slowly opens up over weeks Creep, not lack of strength Thicken the section or choose a material that creeps less; see Creep and fatigue

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?