kapy academy

Layers splitting apart

14 min readUpdated Nov 2026

You have an ABS box that cracked along a layer before you even took it off the plate, or a PLA bracket that looked perfect and snapped cleanly along a layer the moment it took a load. In both cases the weld between layers has failed (delamination). Every FDM part is weaker across its layers than along them (Layer adhesion and anisotropy), but a bond that comes out weaker than it should be can be fixed. Read the break first: each way of splitting leads to a different fix.

The same wall hook printed upright, on the left, and lying down, on the right, hung on the wall with the same load: in the upright one the layers are edge-on to the force, a crack opens between two layers at the root of the arm and it snaps cleanly; the lying one, with its layers along the arm, bends and holds. Then both go back to the bed and are printed again, layer by layer
Same hook, same plastic, same load. Printed upright, the arm grows as a tower and the force pulls two layers apart at its root: the break is flat and smooth, the face of a layer. Printed lying down, the layers run along the arm and the load pulls on the beads. Bending is exaggerated and the layers are drawn thicker.

How much heat reaches the weld

The new bead has to reheat the surface of the bead below until the polymer chains can move and diffuse across the joint. The weld is as wide as the molten neck left between the two. Anything that takes heat away before that happens narrows the neck: plastic that leaves the nozzle cold, strong air on the freshly laid bead, or a long wait since the layer below went down.

weld neckgap between beadswelded hotwelded cold
The same wall welded hot and welded cold. With heat to spare, the neck between beads is wide; with cold plastic it is narrow, leaves gaps at the cusps, and the crack follows the joint.

Three factors decide the weld, and every setting acts only through them:

  1. The real temperature of the plastic as it leaves the nozzle. That is the heat the new bead brings to remelt the one below.
  2. How fast the surface below has cooled. The part cooling fan, drafts and the chamber air carry that heat away.
  3. The time since the layer below was laid. The longer the layer time, the colder the surface the new layer has to weld to.

The temperature you set is not the temperature of the plastic coming out. At the flow limit, the plastic spends very little time in the melt zone and leaves colder than the screen says. A part printed at the hotend's flow ceiling can have weaker layers than the same part printed more slowly at the same temperature. Lower "Max volumetric speed" in the filament profile, or raise the temperature by 5–10 °C; where that ceiling comes from is in Volumetric flow sets the speed.

The nozzle material matters too. A hardened steel nozzle conducts heat worse than brass and needs 5–10 °C more or 10–20 % less flow: fit one to print carbon-fiber filament, keep the same profile, and you get weak layers. Tell the slicer which nozzle is fitted (Nozzles: size and material).

The neck also depends on how hard the bead is squashed into the one below. A slightly low "Flow ratio", or a layer height above 75 % of the nozzle diameter, cuts the contact between beads even when no gaps show: calibrate the flow and stay between 25 and 75 % of the nozzle. Thinner layers are no fix either: there are more joints and each layer brings less heat, so they bond no better (Layer height and line width).

Read the break before you touch anything

Each way of breaking points to a different family of causes. Identify yours first.

airbedthermal crackforceflat facesnapped under loadlayer Npause / swapone weak height
Three ways to split between layers: a crack that opens by itself in the upper half on the side facing the air, a flat break along one layer when the load crosses the layers, and a crack at the one height where something interrupted the print.

A. Cracks that open by themselves. They appear during the print or minutes to hours afterwards. This is stress from thermal shrinkage, typical of ABS, ASA, PC, PA and their blends. They usually sit in the upper half of tall parts, often on the face turned toward the door, the auxiliary fan or the room. It is the same stress that lifts corners in Warping and lifting corners, except that here it breaks the weakest layer instead of peeling the base.

Cracks opening along the layer lines in the upper half of a printed wall; the layers below are still welded (generated illustration)
Cracks opening along the layer lines in the upper half of a printed wall; the layers below are still welded (generated illustration)

B. A part that looks fine and snaps cleanly along a layer under load. The fracture face is flat, smooth or glossy, and you can make out the rows of beads. If the face is fibrous and torn, the bond held: the part was overloaded (Reading a failed print). A break along a layer takes two things: a thin weld (cold, too much fan, damp filament, too much speed) and a load that crosses the layers.

C. A weak plane at one particular height. The part always opens at the same layer, and something happened at that height: a pause, a spool running out or a color change, a material change, a step in cross-section, or a partial clog. Find that layer in the slicer preview and check what happens there; the causes are in the section "A weak layer at one height", further down.

Two failures look like this and are not. Visible gaps between beads all over the wall, even with thin layers, are under-extrusion (Extrusion problems). A sideways step at one height is a layer shift (Layer shifts and spaghetti).

Cracks in ABS, ASA, PC and PA

These materials print at 240–290 °C, turn rigid well above room temperature and shrink by roughly 0.5–0.8 % (ABS, PC), 0.4–0.7 % (ASA) and 1–2 % (unfilled PA). Each new layer goes down on layers that are already cold and rigid, and as it cools it shrinks and pulls on the joint below. Higher up, away from the bed, the part no longer gets the heat conducted up from it and is more exposed to drafts and the auxiliary fan, so the temperature drop is larger; that is why the crack appears in the upper half and along the weakest weld. PLA and PETG shrink by roughly 0.2–0.5 % and also turn rigid at a much lower temperature, so they build up little stress and rarely crack this way.

The enclosure. Close the door or the lid and let the chamber warm up before the first layer. A passive enclosure heated by the bed is usually enough for ABS and ASA; PC does better with a heated chamber, and PA-CF needs one. As of late 2026, machines such as the Bambu H2D heat the chamber to 65 °C. The hardware is covered in Enclosures and heated chambers.

Air from one side. If your printer has an auxiliary fan (X1, P1S, H2D and the like), switch it off: Bambu's profiles leave it at 0 % for everything except PLA and TPU. On the same machines, keep the chamber exhaust fan low, so it filters the air instead of dumping the heat. On an open printer, move it away from the air conditioning and from window drafts. A crack on only one face points to a draft from that side.

The part cooling fan. Current profiles run it at 10–30 % for ABS and PC, 15–30 % for ASA, up to 80 % on overhangs and bridges, and 0–30 % for PA, always inside an enclosure. Switching it off does not help: overhangs droop and the bond gains nothing. A short burst over a small overhang will not crack ABS; a whole layer at 80 % on a large part can (Overhang and bridge settings).

The temperature. The top half of the nozzle range (ABS 240–280 °C, ASA 240–270 °C, PC 260–290 °C) gives welds that stand up better to the same stress.

With tall, thin walls, ABS cracks sooner. Thicker walls, fewer sharp inside corners or the part split into shorter sections (Splitting large parts) reduce the stress. Printing ABS in an enclosed printer calls for filtration or ventilation (Emissions and ventilation).

Parts that snap along a layer

PLA. The fan at 100 % gives the best finish, but on a functional part it costs layer adhesion. In order: raise the nozzle temperature by 5–10 °C toward 230 °C (range 190–230 °C, typical profile 215 °C) and lower the speed or the max volumetric speed; then try the part cooling fan at 50–70 % on layers without overhangs. Do not pick the temperature by eye: print a tower and break it (Temperature towers and retraction tests).

Silk PLA and heavily filled PLAs bond worse than plain PLA because of their additives; the Bambu wiki singles out silk, especially when it is printed too fast or too cold. Print them hotter and slower, and keep them out of load-bearing parts (PLA and its variants).

PETG. PETG printed with PLA settings is the textbook case of weak layers. Fan at 30–60 % (50–90 % on bridges), nozzle between 230 and 270 °C starting at 245 °C; with PETG HF, fan at 10–40 %. A PETG wall is glossy anyway, so do not trust its looks: the sign of too much fan is a part that snaps along a layer with a smooth, glossy fracture face.

Layer time. On a large layer, the one below spends minutes cooling before the next arrives, and the weld comes out colder. The opposite failure, the tiny layer with no time to cool, is covered in Speed and cooling. Every part you add to the plate lengthens the layer time: a large functional part welds better printed on its own. Sequential printing only works for parts shorter than the clearance under the carriage or gantry (Many parts on one plate).

Orientation matters most, and it costs nothing. For design, assume the part is half as strong in Z as in XY, or 30 % if the material is fiber-filled, and orient it so the main load runs along the beads (Layer adhesion and anisotropy). With long layer times, lots of fan, damp filament or ABS on an open printer, a real part drops to 20–40 % and fails without warning. Lay hooks, clips and brackets down (Orientation and overhangs).

If the part is already printed, annealing relieves stress and in some plastics may improve the bond a little, at the cost of distorting the part; it does not fill voids or make up for poor orientation (Annealing and strengthening).

Damp filament

Absorbed water does two things in the melt zone. It cuts the polymer chains (hydrolysis) in PLA, PETG, PC and polyamides: the molecular weight drops, the plastic turns brittle and diffuses worse across the joint, even if you never see a single bubble. And it flashes to steam: the bead comes out porous, the nozzle hisses or pops softly, and the surface is rough with fine bubbles, with the voids right at the weld. What gives it away is the combination: weak layers, stringing and a rough skin all at once.

PC, PA (filled and unfilled), TPU and PVA always need drying; PLA, PETG, ABS and ASA benefit from it. Left in the open, nylon (PA) takes up enough water to ruin a print in a few hours or days.

Dry before you change any setting; temperatures, times and the limits of built-in dryers are in Drying and storing filament. Do not raise the temperature to make up for damp filament: more heat speeds up hydrolysis, the steam is still there, and all you gain is stringing and oozing.

A weak layer at one height

A pause for magnets or nuts. During the pause the last printed layer cools completely and the next one welds to cold plastic. Keep pauses short, keep the printer closed, and put the pause where the load does not cross that layer (Embedding magnets and nuts mid-print).

A filament change or a spool running out. A long purge or a failed load leaves the part waiting. In a multicolor print with many swaps per layer, the layer time stretches sharply and a large ABS part can crack (Multi-material failures).

A material change. Two materials that do not bond will come apart at the change: PLA and PETG weld poorly to each other, which is exactly why PETG works as a support interface under PLA. A functional multi-material part needs compatible pairs or mechanical interlocks (Functional multi-material parts).

A step in cross-section. When a thin column widens into a plate and the part always breaks at the junction, two causes add up. The geometric one: the sharp inside corner concentrates stress right where the bending moment peaks. The thermal one: on the column, the slicer applies the minimum layer time, slows down and turns the fan up to full, so the column is what welds cold. Round or chamfer the junction and, if the column carries load, raise its temperature or lower the fan over that stretch.

A partial clog or heat creep. A band of thin, gappy layers at that height is under-extrusion, not a weld failure (Extrusion problems).

When it fails

Symptom, cause and fix
Symptom Cause Fix
ABS, ASA or PC cracked during the print, in the upper half, on one side Draft, auxiliary fan, open door or high fan on a large layer Close the door, auxiliary fan at 0 %, part cooling fan at 10–30 %, warm chamber (Enclosures and heated chambers)
Functional PLA part snapped cleanly along a layer Cold weld: fan at 100 %, too much speed Raise 5–10 °C, slow down, fan at 50–70 % without overhangs, reorient (Orientation and overhangs)
PETG part snapped cleanly along a layer Too much fan Fan at 30–60 %, start at 245 °C (Speed and cooling)
Weak layers with hissing, bubbles and a rough skin Damp filament Dry it first (Drying and storing filament)
Weak layers since you swapped brass for hardened steel Steel conducts heat worse than brass Raise 5–10 °C or lower flow by 10–20 % (Nozzles: size and material)
Weak layers only at top speed At the flow limit, the plastic leaves colder than the setting Lower "Max volumetric speed"
Always opens at the same height Pause, filament change, material change or step in cross-section Check that layer in the preview (section "A weak layer at one height")
Silk PLA that cracks Additives that weaken the bond Hotter, slower, and never for load (PLA and its variants)
Visible gaps between beads all over the part Under-extrusion, not a bond failure Extrusion problems

How to test it

Print a temperature tower or a vertical test wall in the part's material, nozzle and profile, and break it by hand, bending it against the layers. A smooth, glossy fracture face is a cold weld; a fibrous, torn face means the bond holds (Temperature towers and retraction tests). Change one thing per test print and always break it the same way.

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?