kapy academy

Speed and cooling

19 min readUpdated Nov 2026

A slicer does not print "at a speed": it gives every line type its own speed and its own acceleration, caps them at what the hotend can melt and, after that, the filament profile can slow a whole layer down and raise the fan so that layer cools. To start with, keep the speeds in your printer maker's profile, because on a current machine the real ceiling is volumetric flow. Tune only the outer wall for looks, the minimum layer time for small parts and the fan for the material, and change one thing per test print.

One speed per line type

Slicer labels are quoted as they appear on screen at the end of 2026. Speeds live in the process profile; cooling and layer time live in the filament profile (Printer, filament and process profiles).

Every slicer works with the same set of line types: outer wall, inner walls, sparse infill, internal solid infill, top surface, gap fill, small perimeters, bridges and overhangs, support, first layer and travel. These are their values in three stock profiles, with a 0.4 mm nozzle and 0.20 mm layers:

Speed per line type in mm/s, stock profiles at the end of 2026
Line type Bambu X1C "0.20mm Standard" Prusa CORE One "0.20mm SPEED" Prusa CORE One "0.20mm STRUCTURAL"
Outer wall 200 170 50
Inner walls 300 170 70
Sparse infill 270 200 120
Solid infill 250 200 140
Top surface 200 100 80
Gap fill 250 120 60
First layer 50 45 45
Travel 500 350 350
Bambu X1C 0.20mm StandardPrusa CORE One 0.20mm SPEEDout of reach (flow ceiling)Outer wall200170Inner walls300170Sparse infill270200Solid infill250200Top surface200100First layer504515 mm³/s≈167 mm/s21 mm³/s with a 0.45 × 0.20 mm bead≈233 mm/s050100150200250300Speed (mm/s)
Each line type has its own speed, but the filament's flow limit puts a common ceiling over all of them: anything above that line never prints at the speed you set.

The outer wall is the only line you see and the one that sets the part's dimensions. So it runs slower and, above all, with less acceleration: less ringing (the ripples that follow every corner), steadier pressure through the corners and a cleaner seam. Inner walls and infill are hidden, so they run as fast as flow allows. The top surface prints slower so the skin closes flat over the infill (Top surfaces). The first layer goes slowly so the bead has time to grip the bed (The first layer and bed adhesion). Bridges and overhangs have speeds of their own, covered in Overhang and bridge settings.

Holes and small contours are short on each layer and full of direction changes. Bambu Studio and Orca print them with "Small perimeters" at 50 % of wall speed when the contour is smaller than the radius in "Small perimeters threshold". Set it to 0 and the slicer uses a built-in radius. A short contour closes in under a second and, with that many corners, the nozzle would never reach full speed anyway.

Prusa's STRUCTURAL profile is telling: the maker ships a separate setup for functional parts, with walls at 50–70 mm/s and lower wall accelerations, so each bead goes down slower and with more even pressure. What that gains and costs you is in Speed against finish and strength.

These numbers do not carry over from one machine to another. An outer wall at 200 mm/s is reasonable on an enclosed CoreXY and a bad idea on a legacy bedslinger, which runs walls at 40–80 mm/s and accelerations of 500–1,250 mm/s². A modern bedslinger with input shaping and pressure advance handles walls at 150–200 mm/s without trouble. Always start from the maker's profile for your machine.

Flow sets the ceiling

The speed ceiling is the hotend's flow: speed = flow / (line width × layer height) (Volumetric flow sets the speed). The filament profile sets a maximum volumetric flow, and the slicer silently caps any line type that would exceed it. With Bambu PLA Basic, limited to 21 mm³/s on the X1 and P1, a 0.45 × 0.20 mm bead allows about 233 mm/s at most. The X1C profile's sparse infill at 270 mm/s and inner walls at 300 mm/s, both 0.45 mm wide, actually print at about 233. Solid infill is 0.42 mm wide, and its 250 mm/s lands right on the ceiling. Prusament PLA is limited to 15 mm³/s: about 167 mm/s, so the CORE One SPEED profile's infill at 200 mm/s actually prints at about 167. With PETG the ceiling drops a long way: Bambu PETG Basic is limited to 8 mm³/s, about 89 mm/s with the same bead.

The profile speed is a maximum. Short runs between corners never reach it, because the nozzle spends them accelerating and braking (you will see this in What a slicer does). That is why each line type also carries its own acceleration:

Acceleration per line type in mm/s², stock profiles at the end of 2026
Line type Bambu X1C "0.20mm Standard" Prusa CORE One "0.20mm SPEED" Prusa CORE One "0.20mm STRUCTURAL"
Default 10,000 3,000 3,000
Outer wall 5,000 3,000 1,500
Inner walls 10,000 6,000 2,500
Sparse infill 10,000 7,000 6,000
Top surface 2,000 2,000 2,000
First layer 500 500 500

Lowering the outer wall's acceleration cleans up ringing more than lowering its speed (Acceleration, resonance and input shaping). Cura's generic profile leaves "Enable Acceleration Control" off, so whatever acceleration the firmware is set to wins; your printer's profile may turn it on.

Minimum layer time

Each layer has to cool below the material's softening temperature before the next one rests on it. A large layer takes minutes to print, so it is cold by the time the nozzle comes back. A layer at the tip of a cone, on a 5 mm pin or at the top of a thin tower prints in one or two seconds: the nozzle comes back over plastic that is still soft, drags it, and heat builds up layer after layer until the tip melts, bends or curls.

The same cone printed with minimum layer time (left) and without it (right): the tip had no time to cool and melted into a blob (generated illustration)
The same cone printed with minimum layer time (left) and without it (right): the tip had no time to cool and melted into a blob (generated illustration)

The slicer handles it like this: if a layer's estimated time is below a threshold, it slows every move in that layer proportionally until the layer takes as long as the threshold, never dropping below a minimum speed. In Bambu Studio and Orca the switch is "Slow printing down for better layer cooling".

Default minimum layer time, end of 2026
Slicer Setting Stock values
Bambu Studio and Orca "Slow printing down for better layer cooling" (on), "Layer time" under "Max fan speed threshold", "Min print speed" PLA 4 s, PETG Basic 12 s, ABS and ASA 3 s, PA and PC 2 s; minimum speed 20 mm/s for PLA, 10 mm/s in Bambu's generic profile
PrusaSlicer "Slow down if layer print time is below", "Min print speed" CORE One: Prusament PLA and PETG 8 s, ASA and PC Blend 10 s; MK4S: PLA 6 s, PETG 7 s; minimum speed 15–20 mm/s
Cura "Minimum Layer Time", "Minimum Speed", "Lift Head" 5 s, 10 mm/s, "Lift Head" off

In Bambu Studio and Orca the slowdown threshold is the same "Layer time" that drives the fan to maximum, so on a short layer both happen at once.

The limit of this mechanism is the minimum speed. A 5 mm pin with three 0.45 mm walls has about 35–40 mm of path per layer: about 0.2 s at 200 mm/s. Even slowed to the 20 mm/s minimum, the layer lasts only about 2 s, short of PLA's 4 s. The fixes, in order:

  1. Print two or more copies spaced apart, so each layer lasts longer and each part cools while the nozzle prints the others (Many parts on one plate).
  2. Make sure the fan is at maximum on those layers (next section).
  3. In Cura, turn on "Lift Head": the nozzle moves away and waits until the time is up.
  4. As a last resort, add a sacrificial tower beside the part to lengthen each layer.

Pushing the minimum speed even lower only trades a melted tip for blobs: at a few mm/s the nozzle oozes.

The slowdown has a side effect: it changes the outer wall's speed over a band of layers, and on silk, glossy or dark filaments that shows as a change in sheen or a stripe. Bambu Studio and Orca have an option, off by default, that keeps the outer wall at its speed and slows only the rest (its label is in the fault table below). Use it when the stripe bothers you more than the heat (Wall marks: ringing, VFA and Z-banding).

The part-cooling fan

The part-cooling fan, also called the layer fan, blows on the freshly laid bead so it sets where it lies: sharp corners, crisp fine detail, overhangs and bridges. The price is that the layer below is colder when the next bead arrives, and the weld between layers comes out narrower. Every cooling setting is a balance between the two (Layer adhesion and anisotropy).

weld neckgap between beadshot beadcold bead
With more air, the bead below is colder when the next one lands and the weld neck narrows: that is why materials that shrink a lot print with little fan.

In Bambu Studio and Orca the fan follows a curve with two layer-time thresholds. If the layer lasts longer than "Min fan speed threshold › Layer time", the fan runs at the minimum "Fan speed"; if it lasts less than "Max fan speed threshold › Layer time", at the maximum; in between, it interpolates by layer time. "Keep fan always on" stops it dropping to 0.

Part-cooling fan curve in Bambu's profiles, end of 2026
Material Minimum → maximum Minimum if the layer lasts more than Maximum if it lasts less than
PLA 100 % → 100 % 100 s 4 s
PETG Basic 10 % → 40 % 30 s 12 s
ABS 10 % → 80 % 30 s 3 s
ASA 10 % → 80 % 35 s 3 s
PC 10 % → 60 % 30 s 2 s
PA 0 % → 60 % 4 s 2 s

On a large ABS part, with layers lasting several minutes, the fan sits at 10 % and only rises on the small layers.

Max fan speed threshold (PETG, 12 s)Min fan speed threshold (PETG, 30 s)Fan (%)050100PLAPETGABSSpeed (% of the set value)0100PLAslowdown to reach the minimum layer timestill too short; print copiesMin print speed0410203040Estimated layer time (s)
Fan and speed both follow how long each layer takes: short layers get more air and are slowed down, until the minimum speed leaves no room to slow further.

PrusaSlicer and Cura follow the same idea under other names (Orca, Bambu Studio, PrusaSlicer and Cura). PrusaSlicer has "Enable auto cooling", "Min" and "Max" fan speed, "Enable fan if layer print time is below" and "Keep fan always on". On the CORE One, Prusament PLA runs at 85–100 % below 40 s; PETG at 30–60 % below 20 s; ASA at 20–25 %; PC Blend at 15–25 % below 35 s. On the MK4S, PLA runs at 70–100 % below 17 s. Cura has "Regular Fan Speed", "Maximum Fan Speed" and "Regular/Maximum Fan Speed Threshold" at 10 s, with the fan at 100 %.

The first layers print with the fan off, then it ramps up. Bambu Studio turns it off for the first layer with PLA and TPU and for the first three with everything else ("No cooling for the first"), and brings it to maximum at the layer set in "Full fan speed at layer". Prusa's profiles turn it off for the first layer with PLA and reach maximum on the third; with PETG they turn it off for the first three and reach maximum on the fifth; with ASA they turn it off for the first four. Cura starts with "Initial Fan Speed" at 0 % on the first layer and reaches regular speed on the second ("Regular Fan Speed at Layer" = 2). The first layer needs its heat to grip the plate, and air at the edges of a hot bed is where warping starts (Warping and lifting corners).

A percentage is not an airflow. 100 % on a legacy bedslinger with a small blower on one side moves far less air than 100 % on a machine with a large blower and ducts on both sides of the nozzle, and on the first one the side of a round part away from the blower cools worse. That is why a percentage copied from another printer's profile tells you little. The overhang and bridge fan, which runs higher than the layer fan wherever the slicer detects an overhang, is covered in Overhang and bridge settings.

Auxiliary fan and chamber fans

The auxiliary fan is a large fan mounted on the side of the chamber in some enclosed CoreXY machines, such as Bambu's X1C, P1S or H2 series; other makers fit similar side fans. It blows sideways across the whole plate. Bambu's profiles run it at 70 % for PLA and TPU and at 0 % for everything else. With PLA it pulls heat out of the chamber and cools large top faces. With ABS, ASA, PC and PA it stays off because air from one side cools that side before the rest, and the part warps or cracks right there. In Bambu Studio and Orca you enable it in the printer profile with "Auxiliary part cooling fan" and set it in the filament profile with its own "Fan speed". Cura has no dedicated auxiliary fan setting; its "Build Volume Fan Speed" drives the chamber fan on printers that have one.

Chamber and exhaust fans do different jobs depending on the material. With PLA and PETG they pull heat out so the chamber does not get so hot that the air can no longer cool the hotend's heatsink and the filament softens before the melt zone (heat creep, which ends in a clog), and so thin walls do not sag. With ABS, ASA and PA they run slowly and push the air through the filter, keeping the chamber warm and the air clean: Bambu's profiles turn on "Activate air filtration" for ABS, ASA and PA, with the exhaust at 70 % in Bambu's generic profile. On the Prusa CORE One, with PLA you open the top vent by hand and raise the chamber fans, and the printer warns you if the chamber overheats.

The door rule: on an enclosed printer, leave the door or lid open with PLA, PVA and TPU once the bed goes above about 45 °C, and with PETG once it goes above about 70 °C. Close it for ABS, ASA, PC and PA. The chamber itself is covered in Enclosures and heated chambers; what the room breathes, in Emissions and ventilation.

When to turn cooling down

Part-cooling fan by material
Material Part-cooling fan Overhangs and bridges Door or chamber
PLA 100 % 100 % door open
PETG 30–60 % 50–90 % door open
PETG-HF 10–40 % 90 % door open
PCTG 20–50 % — door open
ABS 10–30 % up to 80 % closed
ASA 15–30 % up to 80 % closed
PC 10–30 % — closed
PA and fiber-filled PA 0–30 % — closed or heated
TPU 50–100 % — door open
PVA and BVOH 100 % — door open
PEEK and PEI 0 % — industrial printer

Turn cooling down when the material shrinks a lot, as ABS, ASA, PC and PA do: with the fan blowing on a large part, each layer arrives cold at the next, the weld between layers comes out narrow and the material's shrinkage pulls it open. Turn it down with PETG too: at full fan it welds poorly between layers and the part breaks along them. And turn it down when a functional part breaks along a layer: if it is PLA, first raise the nozzle temperature and lower the speed; then try the part-cooling fan at 50–70 % on layers without overhangs (Layers splitting apart).

Turn it up, or keep it high, on small layers, fine tips and text, on overhangs and bridges, and with PLA in a warm chamber.

:::note{kind="warn" title=""Turn the fan off for ABS" is outdated advice"} Current profiles print ABS, ASA and PC with the part-cooling fan at 10–30 %, with more on overhangs and bridges, inside an enclosed printer. With the fan at 0, overhangs and fine detail droop and you gain nothing in return. What cracks ABS is a draft: an open door, the auxiliary fan, or a high fan on a large layer. :::

When it fails

Symptom, cause and fix
Symptom Cause Fix
Tip of a cone or pin melted, bent or blobby The layer is shorter than the minimum time even at minimum speed Print several copies; fan at maximum on those layers; "Lift Head" in Cura
You raise the speed and the time does not change You are at the volumetric flow ceiling Bigger nozzle or high-flow hotend (Volumetric flow sets the speed)
Change in sheen or a stripe on the outer wall, a few millimeters tall The cooling slowdown changed the outer wall's speed "Don't slow down outer walls" (Bambu Studio, Orca)
Ringing after corners on the outer wall Acceleration too high for that wall Lower the outer wall's acceleration before its speed (Wall marks: ringing, VFA and Z-banding)
PETG part that breaks along the layers Too much fan Part-cooling fan at 30–50 % and a few degrees more on the nozzle
ABS or ASA cracked on one side, or corners lifting mid-print A draft: auxiliary fan, open door or high fan on a large layer Auxiliary at 0 %, door closed, part-cooling fan at 10–30 % (Warping and lifting corners, Layers splitting apart)
Corners of the first layers lifting Fan on too early No fan for the first 1–3 layers, then a ramp
PLA clogging or thin walls sagging partway through a long print in an enclosed printer Chamber too hot, heat creep Open the door or lid, turn the chamber fans up (Hotends and how much they can melt)
Small overhangs and corners curling in PLA Not enough air reaches that side Check the fan %, the duct and the auxiliary; if one side comes out worse than another, the problem is how the air is distributed, not a slicer setting
Holes or bumps in a top layer over infill Too little cooling on the top layers or too few top layers Top surfaces

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?