A brim, mouse ears and a raft are plastic you print to throw away. A brim and ears add contact with the plate where the part is short of it; a raft lifts the part off a surface that cannot support it. None of them fixes a bad first layer (The first layer and bed adhesion). With a clean plate, almost no PLA or PETG part needs any of them. Use a 5 to 8 mm brim for small footprints and tall, narrow parts, ears when only the corners lift, and a raft almost never.
What each one fixes
A part comes off the plate for one of two different reasons, and it pays to tell them apart before you pick a remedy. The first is too little contact: the part is small, or it stands on separate pads or on a thin edge, and the sideways push of the nozzle knocks it loose or, if it is tall and narrow, levers it over. The second is corners peeling up: the part stuck fine, but the layers above shrink as they cool and pull the corners of the footprint upwards. That is warping, and the mechanism is explained in Warping and lifting corners.
Both start at the outline. Peeling concentrates the force at the front of the bond, like peeling tape from one end. That is why the bonded area next to the outline does the holding, not the area in the middle.
A brim is a set of concentric loops in the first layer, fused to the part's outline, that extend the contact outwards all the way round. It works against peeling because it moves the front of the bond several millimeters away from the outline. Being a single layer thick (0.20 mm with a 0.4 nozzle), it is too thin and flexible to warp on its own: it only anchors. Nor is it a rigid foot, because a 0.2 mm sheet bends. On a tall part it resists tipping because the part can only fall by peeling up a longer strip further from its base, not because it moves the point the part pivots on. The center of mass still sits over the same footprint, and if the base tears away from the brim, the part falls all the same.
Mouse ears are discs of brim placed only at the corners and sharp points, which is where peeling starts on large parts. They anchor the critical points for a fraction of the plastic and the cleanup, and they leave long straight edges clean.
A raft is a thick sacrificial grid under the whole part; the part prints on top of it, separated by a small air gap. At the outline it grips no better than a brim. What it gives you is a base other than the plate: the part never touches it. It is worth it in very few cases, and in exchange the underside comes out rough and the part's first layer is less accurate. All of this is FDM; in resin, the raft is the base that carries the supports and is covered in Orienting and supporting resin prints.
A skirt is a set of loops around the part that do not touch it. They prime the nozzle and let you check the first layer before the part starts, but they do nothing for adhesion. As of late 2026, Bambu's profiles ship with "Skirt loops" at 0, Orca's base value is one loop 2 mm from the part, and in Cura "Skirt" is one of the four options under "Build Plate Adhesion Type". A skirt several layers tall ("Skirt height", or "Draft shield" in Orca, PrusaSlicer and Cura) shields ABS from drafts; Warping and lifting corners covers it.
Brims: when and how wide
Add a brim in four cases:
- Little contact area: a part standing on a ring, on legs or on a thin edge.
- Tall, narrow parts: a column, a fin standing on edge.
- High-shrinkage materials (linear shrinkage: ABS 0.5–0.8 %, PC 0.5–0.8 %, ASA 0.4–0.7 %, unfilled nylon 1–2 %) on footprints longer than a few centimeters.
- TPU parts with a small footprint, which the nozzle tends to drag along.
| Slicer | Setting | Default |
|---|---|---|
| Bambu Studio (Bambu profiles) | "Brim width" | 5 mm |
| Cura | "Brim Width" | 8 mm |
| OrcaSlicer, Bambu Studio | "Brim type" = "Auto" | usually no brim below about 5 mm; 18 mm at most |
| All | width for tall parts and small footprints | 5–8 mm |
In Bambu Studio and OrcaSlicer, leave the brim on "Auto": it decides from the part's shape and material, and it gets it right more often than any fixed value. It works out the width from how tall the part is compared with the size of its base, the print speed (faster means wider) and the material. A squat PLA box gets no brim; a tall, narrow part gets one. With PETG the result comes out twice as wide as with PLA, and with TPU half as wide. On high-shrinkage materials the cap can sit below 18 mm on small parts. That is how both slicers behave today; it can change in any release.
Going past about 10 mm by hand rarely holds any better. Peeling is stopped at the front of the bond, and once that front is out of the zone the part pulls on, more plastic only means more to clean up. "Auto" goes up to 18 mm on very tall parts printed fast; if you think you need more than 10 mm by hand, the problem is usually the orientation or the first layer.
Use an outside brim only, "Outer brim only". "Inner brim only" and "Outer and inner brim" add loops inside holes: they are hard to remove and leave marks on the hole walls, which almost always matter, such as a bearing seat or a screw hole. Keep the inner brim for when what lifts is an inner outline, like that of a large frame. In Cura, the brim is set with "Brim Width" or "Brim Line Count", and "Brim Location" picks outside, inside or both; check the label in your version.
In Bambu Studio and Orca, "Brim type" = "Painted" lets you paint where the brim goes: a long part can have one only at the end that lifts. PrusaSlicer has four types (no brim, outer, inner, both) and no painting.
If you fill the plate, leave each part room for its brim. Two brims that touch fuse into one sheet that does not come apart cleanly; the spacings are in Many parts on one plate.
Mouse ears: a brim only where it is needed
Ears are the right call for:
- Large, flat parts in materials that warp, when only the corners lift.
- Parts with long faces that must stay clean: a visible edge, a sliding face, a flange that seats against another.
- Parts where cleaning off a full brim would take longer than printing them.
On large ABS parts they work better than a full brim because at a corner the shrinkage of two walls adds up and the peel front is shorter, and that is where anchoring pays off most. Rounding the corners of the footprint in plan helps for the same reason and leaves nothing to clean; the right radius is covered in Warping and lifting corners.
| Slicer | How | Settings |
|---|---|---|
| OrcaSlicer | "Brim type" = "Mouse ear", automatic on corners; or "Painted" with the ear tool | "Brim ear max angle" 125°, "Brim ear detection radius" 1 mm |
| Bambu Studio | only with "Brim type" = "Painted": ear tool, automatic on corners or by hand | ear diameter in the tool |
| Cura | not built in; there is a Marketplace plugin | — |
| PrusaSlicer | not built in | model them |
Orca puts an ear on every corner sharper than "Brim ear max angle", after simplifying the outline with the detection radius. In Bambu Studio the ears do not show until you slice.
Modeled ears work in any slicer and are the way to go if other people will print your part. Model discs about 10–15 mm across and one or two layers thick (0.2–0.4 mm); thicker than two layers and they no longer snap off cleanly. Center them on each corner so they overlap the part by a few millimeters. You can join them to the part or leave them as a separate body that touches it.
Rafts: the few cases that justify one
The raft used to be the cure for badly leveled beds and glass that nothing would stick to. A modern bedslinger or an enclosed CoreXY comes with mesh leveling and a textured PEI plate, and many probe with the nozzle itself, which also sets the Z offset; those causes are gone. On a legacy bedslinger without a mesh it can still make sense. The raft's costs, on the other hand, are still there:
- The underside takes on its texture.
- The part's first layer prints onto plastic across an air gap and sags slightly between the raft's beads, so it is less accurate.
- It costs material and time, and if the gap is wrong, it is hard to separate.
A raft does not spread shrinkage stress either: the part shrinks by the same amount on top of it. Nor does it rescue a material that will not stick to your plate, because the raft is printed in that same material and does not stick either. Polypropylene needs a PP sheet or packing tape (see Polypropylene); for everything else, surfaces and adhesives are in Bed prep for each material.
It is justified in these cases:
- A base that is not flat, or that has tiny contacts at different heights: scanned or organic parts, a part on several small feet.
- A bottom edge that cannot have elephant's foot and is not a functional face. That is rare.
- Tiny parts on a worn plate, as a one-off workaround. The fix is to replace the plate: Bed and motion upkeep.
- As a base for supports. Slicers put it in the support panel and it shares their interface settings.
| Setting | OrcaSlicer / Bambu Studio | PrusaSlicer | Cura |
|---|---|---|---|
| Turning it on | "Raft layers" (0 = no raft); use 2–3 | "Raft layers" | "Build Plate Adhesion Type" = "Raft" |
| Gap to the part | "Raft contact Z distance" 0.1 mm | "Raft contact Z distance" 0.1 mm (Prusa profiles: 0.1–0.25 depending on layer height) | "Raft Air Gap" 0.3 mm, with "Initial Layer Z Overlap" 0.15 mm |
| Margin around | "Raft expansion" 1.5 mm | "Raft expansion" 1.5 mm | "Raft Extra Margin" 15 mm |
| Raft first layer | "First layer expansion" 2 mm, "First layer density" 90 % | — | — |
The gap does the same job as in a support interface: it is what lets the part come away. Too small and the raft welds on; too large and the part's first layer droops. Adjust it in 0.05 mm steps. In Orca, if "Support top Z distance" is at 0, the slicer ignores the raft gap.
A zero-gap raft needs a multi-material printer (AMS, MMU, toolchanger or IDEX) and an interface in a second material that does not bond to the part: PETG under PLA, PLA under PETG, or a soluble material. The underside comes out like a support interface face: smoother than on a normal raft, without the plate's finish. How to assign the interface material is in Support settings; which materials work, in Support materials.
In PrusaSlicer and Cura, a raft prints without a brim: PrusaSlicer says so in the "Brim width" tooltip, and in Cura they are mutually exclusive options of "Build Plate Adhesion Type". If you need more grip, widen the raft's first layer.
Removing them without a mark
The mark a brim leaves depends above all on the gap between it and the part.
| Slicer | Setting | Default |
|---|---|---|
| Bambu Studio (Bambu profiles) | "Brim-object gap" | 0.1 mm |
| OrcaSlicer (base value) | "Brim-object gap" | 0 |
| PrusaSlicer | "Brim separation gap" | 0 (measured from the outline after elephant's foot compensation) |
| Cura | "Brim Distance" | 0 |
Use 0.1 mm. The first-layer bead, 0.50 mm wide with a 0.4 nozzle, squishes out far enough to bridge that gap: the brim still holds the part, but the joint is a thin bridge, not a fused bead, and it breaks along the outline. With a zero gap, the brim and the outer wall are a single bead and a lip is left behind. At 0.2–0.3 mm or more, the brim can end up loose: it grips the plate, not the part.
To take it off, let the plate cool completely: PEI releases the part as it cools and, if you flex the plate, the part pops off on its own. Never force PETG off while hot: on smooth PEI it can tear flakes out of the plate, which is why it goes on textured PEI or with glue stick as a release layer. Take the part off with the brim still on. Then peel the brim by folding it up and back over the outline, starting at a corner; do not pull it outwards flat. Fold ears upwards and tear them off toward the corner.
Run a deburring tool or a blade along the bottom edge to take off whatever is left of the lip; clip ears flush with flush cutters. On visible parts, a 0.5 × 45° chamfer at the base hides the brim line and the elephant's foot in one go (The face on the bed).
A raft comes off by levering from a corner with a spatula or the cutters. If it fights you, the gap was too small for that material: raise it by 0.05 mm next time. Clean up the underside with a blade or sandpaper, and expect the finish of a face printed on supports, not that of a face printed on the plate. Support removal and cleanup covers dressing those marks.
A thin wall or a delicate detail at the base can break as you take the brim off. Leave a gap between brim and part, use ears away from the detail, or paint the brim out of that area.
Solving it in the design
The best brim is a big footprint. Stand the part on its largest flat face (Orientation and overhangs) and round the corners of the footprint in plan. The bottom edge gets a chamfer: a fillet at the base takes away contact (The first layer and bed adhesion). And if other people will print the part with other slicers, model the ears into the part itself.
When it fails
| Symptom | Cause | Fix |
|---|---|---|
| The brim lifts along with the corner | The first layer is not gripping (dirty plate, Z offset, bed temperature) or the material needs an enclosure | Fix the base: The first layer and bed adhesion, Warping and lifting corners, Bed prep for each material |
| The brim stays on the plate and the part has come away from it | Gap too large (0.2 mm or more) | Gap at 0–0.1 mm |
| Brim welded on, lip left when removed | Zero gap | 0.1 mm and deburr |
| Brims of neighboring parts fuse | Parts too close together | More spacing: Many parts on one plate |
| The tall part tips over anyway | Brim too narrow, or the part should be lying down | 8 mm brim, or lay the part down: Orientation and overhangs |
| The part comes loose mid-print and ends up as a nest of spaghetti | Too little brim or a weak first layer, with nobody watching | Catch it in time: Layer shifts and spaghetti |
| The ears do not appear | In Bambu Studio, "Brim type" is not set to "Painted", or you have not sliced yet | Set it to "Painted" and slice |
| Raft welded to the part | Gap too small for the material (PETG and TPU need more), or "Support top Z distance" at 0 in Orca | Raise the gap by 0.05 mm; check the support distance |
| Underside sags on the raft | Gap too large, or the raft's top layer too open | Lower the gap; more density on top |
| Inner brim hard to clean out of a hole | "Outer and inner brim" or "Inner brim only" type | "Outer brim only" |
See also
- The first layer and bed adhesion: why the first bead sticks.
- Warping and lifting corners: why corners lift and what an enclosure does.
- Support settings: the raft's interface and the brim on tree supports.
- The face on the bed: the bottom chamfer and elephant's foot.