kapy academy

Parts that print the wrong size

16 min readUpdated Nov 2026

The part comes off clean, but the shaft will not go into its hole, the lid rocks, or the 100 mm box measures 99.4. Before you touch a setting, work out which kind of error you have: each kind is fixed in a different place, and fixing the wrong one makes everything else worse. A scale error grows with size; an offset is a fixed number of millimeters that makes outside dimensions bigger and inside ones smaller; a local error hits only the base or the round holes, and a geometric one, a single axis or the squareness.

Measure properly before you correct

First know what accuracy to expect: how far a printer of your class drifts and scatters is in Accuracy, precision and repeatability; use your measured figure if you have one. An error inside that band is not a fault: do not chase it, and allow for it when you set the clearances in the design (Real printed clearances).

A single 20 mm calibration cube misleads you for two reasons. Over 20 mm, a 0.3 % shrinkage is 0.06 mm: the same as the repeatability of a hobby calliper or the bump at the seam. And that single number lumps scale, offset and elephant's foot together. Measure at least two sizes, a small one (about 20 mm) and a long one (100 mm or more), in X and in Y, and measure inside dimensions too (a slot or a square hole), not only outside ones.

With the calliper:

  • Measure above the first millimeter: that is where the elephant's foot lives.
  • Measure away from the seam and the corners. At the corners, the pressure still in the nozzle as the head slows down leaves small bulges.
  • Measure away from fuzzy-skin walls: the jaws sit on the peaks and the outside dimension reads large without being an error (Fuzzy skin and textures).
  • Squeeze lightly, and the same every time: plastic gives under the jaws.
  • Take three readings and use the average. A single reading carries the error of how you seated the calliper.

Do not measure small holes with the calliper's inside jaws: the jaws are thin, they touch a chord of the circle instead of the diameter, and read small. Use drill shanks or a set of gauge pins: the hole is the size of the largest one that goes through.

Measure round holes and bosses in X and in Y. If they disagree, one axis is not moving the same distance as the other, because of a belt or a pulley. Shrinkage does not make a vertical hole oval in an unfilled material, as long as you measure away from the seam.

To measure residual warp, rest the part on a flat reference surface (a sheet of glass, a stone worktop, a surface plate) and slide feeler gauges, or sheets of paper of known thickness, under the corners. The thickest one that goes in is the deflection. Measure with the part cold and settled: a part that sat flat on the plate can curl once it is released (Warping and lifting corners).

Write the result down as two numbers per axis: the error on the small part and the error on the long one. That pair is all the diagnosis needs.

Scale or offset: two sizes tell them apart

0measuredscale εoffset 2eoffset 2e02050100error (mm)nominal size (mm)outside dimensioninside dimension
Outside and inside dimensions share the slope (the scale) and separate at the origin (the offset). With two measured sizes you read the slope and the gap directly.

On an outside dimension the error is ε·L + 2e; on an inside one (a slot, a square hole), ε·L − 2e. L is the nominal length, ε the scale error (negative if the part shrinks), e the offset per side (positive if the walls come out fat) and Δ the measured error (measured − nominal). The offset e is doubled because every dimension has two sides. With two sizes, ε = (Δ_long − Δ_short) / (L_long − L_short), and the rest of the error is the offset.

An example in PLA: the 20 mm face measures 20.10 and the 100 mm face measures 99.80. The scale is ε = (−0.20 − 0.10) / 80 = −0.375 %, a normal shrinkage for PLA. At 20 mm that scale predicts −0.075 mm, but you measure +0.10 mm: the offset is 2e = +0.175 mm, about 0.09 mm per side. A 20 mm slot in the same part will come out at around 19.75.

Scale: same sign outside and inside, and it grows with length. It has two causes. The first is material shrinkage, roughly 0.2–0.5 % in PLA, 0.3–0.5 % in PETG, 0.4–0.7 % in ASA, 0.5–0.8 % in ABS and PC, 1–2 % in unfilled nylon and 1.5–2.5 % in PP: over 100 mm, anything from 0.2 to 2.5 mm. The exact figure varies with the brand and with the size of the part. The second is an axis with the wrong steps per millimeter. To tell them apart, print the same test in another material: shrinkage changes with the material, a steps error does not. In an unfilled material, a different scale in X and in Y is not shrinkage either. Fiber-filled materials are the exception: they shrink little along the bead (0.2–0.5 %) and more across it, so they can give different scales in X and in Y depending on how the walls and infill are oriented (Shrinkage and dimensional stability).

Offset: the outside grows and the inside closes by the same amount, whatever the size. The causes are flow set too high (every wall comes out slightly fat), a profile meant for another nozzle or line width, or filament thicker than its nominal 1.75 mm. Over-extrusion also shows on the top face: ridges and nozzle drag marks (Extrusion problems). Set the flow first with the slicer's test (Flow ratio and max flow tests), then correct what remains with contour and hole compensation. The offset left after calibration comes from flow, wall overlap and bead squish. The automatic calibration on Bambu machines measures flow dynamics, which is pressure advance, not the "Flow ratio": it does not replace the flow test.

Where each error is fixed

Shrinkage scale is fixed in the filament profile, because shrinkage depends on the material. OrcaSlicer has "Shrinkage (XY)" and "Shrinkage (Z)" in the filament profile. Bambu Studio has "Shrinkage" in the filament profile, XY only; Z is corrected by scaling the object. PrusaSlicer has "Shrinkage compensation XY" and "Z" under Filament Settings → Advanced. Cura has "Scaling Factor Shrinkage Compensation", split into XY and Z, in the Material section. They do not all expect the same number; there are three conventions: Orca and Bambu want the measured size as a percentage of nominal (99.6 %), PrusaSlicer wants the shrinkage itself (0.4 %) and Cura wants the scale factor (100.4 %). Type 99.6 into Cura and you double the error. Read the field's help text in your version before you fill it in. Do not scale the model on the plate to correct shrinkage: you scale the clearances you designed along with it, and the correction is not stored in the filament profile.

Steps per millimeter are set in the firmware, not in the slicer. On a belt-driven machine with stock firmware and pulleys they are almost never wrong; suspect them after changing a pulley, a motor or the firmware, or on a kit or a self-built machine. Check them by calculation: steps per revolution × microsteps / (belt pitch × pulley teeth). With a GT2 belt, a 20-tooth pulley, a 1.8° motor and 1/16 microstepping, that is 200 × 16 / (2 × 20) = 80 steps/mm. Never tune the steps from a printed part: you would be writing the material's shrinkage into the firmware, and the next spool of a different material would come out wrong.

Once the flow is set, the remaining offset is fixed with the XY compensations. In OrcaSlicer and Bambu Studio they are "X-Y contour compensation" for outer contours and "X-Y hole compensation" for holes closed within the layer, in the quality or precision section of the process profile. They act per side, so halve your diameter error; a positive value makes the feature bigger. Cura has "Horizontal Expansion" and "Hole Horizontal Expansion". PrusaSlicer, as of late 2026, has no separate hole compensation: its "XY Size Compensation" moves contours and holes together. Correct shrinkage first and holes and contours after: XY compensation is a fixed value in millimeters, and if the scale changes afterwards it no longer adds up. To see where you stand, OrcaSlicer ships a "Tolerance" test in its calibration menu.

"Precise wall", in Orca and Bambu Studio, sets the overlap between the outer wall and the inner wall next to it to zero. It matters most with inner/outer wall order, which pushes the outer wall outwards. Turn it on for parts that have to fit. "Precise Z height", in Orca, adjusts the last layers so the top face lands at the modeled height.

Do not chase every fit in the slicer. Compensation applies to the whole profile, and a press fit and a sliding fit on the same part need different clearances: that is a design decision (Choosing the fit: clearance, transition, interference).

Local errors: the base and the holes

Elephant's foot is the flaring of the first layers: the first 0.2–0.6 mm of height, where outside contours spread and vertical holes narrow at the bottom. To measure it, close the calliper over the first layers and then 2–3 mm higher on the same face: the difference divided by two is how far it sticks out on each side. You can also rest the base face on a flat surface and feel for the lip with a fingernail.

Before you compensate, look at the first layer. If it really is over-squished (thin, translucent lines with ridges between them), the problem is the Z offset, which is fixed on the machine (Bed probing and Z offset). Check the bed too: hotter than the filament asks for (above 60–65 °C for PLA), it leaves the base soft and the foot grows. If the first layer is fine, keep the slicer's elephant's foot compensation at its default, 0.075 to 0.2 mm depending on the machine, and add a 0.5 × 45° chamfer to the edge on the bed: the compensation fixes the squish and the chamfer hides the rest. They stack (The face on the bed).

Small round holes print 0.1–0.3 mm tight on the diameter even when outside dimensions are right, because of facets, the bead bulging into the curve and shrinkage (Why holes print small). Look at the export first: with a coarse 12-facet export, a Ø3 mm hole already measures about 2.9 mm across the flats in the file (STL, 3MF or STEP for the slicer). The remedies are exporting at a finer resolution or as STEP, "X-Y hole compensation", "Convert holes to polyholes" in Orca (with "Polyhole twist"), or modeling the hole larger using the calibrated constant. Compensate holes once: in the model, with HOLE_COMP in KapyCAD, or with the slicer's hole compensation, never both.

Horizontal holes, with their axis parallel to the bed, come out oval because the roof sags, and the layer staircase also shortens them vertically. Calibration does not fix that. A horizontal hole up to 6 mm prints clean; between 6 and 10 mm the roof sags 0.1–0.3 mm, acceptable except in a pivot or a precision hole; above 10 mm, draw it as a teardrop or with a flat roof (Designing out supports).

One axis off, or out of square

nominalprintedd1d2skew θXY
A square that is out of square keeps all four sides to size. Only the diagonals give it away: if they differ, X and Y are not at 90°.

If X and Y are not at 90°, a square prints as a rhombus with all four sides correct. Print a square of 100 mm or more and measure both diagonals. For small angles, the skew in radians is the difference between the diagonals divided by the nominal diagonal: θ ≈ (d1 − d2) / (√2 · side). With a 100 mm square and diagonals of 141.6 and 141.2 mm, θ ≈ 0.4 / 141.4 ≈ 0.0028 rad, about 0.16°: the far corner of a 100 mm part shifts by 0.28 mm.

On a bedslinger the usual cause is a gantry that is not square to the frame; on a CoreXY, two belts at different tension or one that has skipped a tooth. Square the frame or tension both belts equally. Klipper ([skew_correction]) and Marlin built with SKEW_CORRECTION (M852) can correct it in firmware. Printers with closed firmware rarely give you access to skew correction; on those, the fix is mechanical only. The full procedure is in Dimensional calibration.

If only one axis is off (X to size and Y short, or a hole that is always oval in the same direction), look on that axis for a slack or worn belt, a pulley with a loose grub screw, or wrong steps. A sliding fit that goes in one orientation and not the other is the same symptom. Belts and pulleys are covered in Bed and motion upkeep.

An error that changes from one print to the next with the same file and the same profile is not a calibration problem. It is repeatability (Accuracy, precision and repeatability) or drift over time: moisture, nozzle wear, belts stretching (When your numbers drift). If you calibrate from a print that came out right by luck, you write that noise into the profile.

Errors in height (Z)

Every height is a whole number of layers. A 10.1 mm dimension with 0.20 mm layers ends up at 10.0 or 10.2; on top of that, the first layer height and variable layer height shift the height at which each feature lands. Design critical heights as multiples of the layer height, or turn on "Precise Z height" in Orca.

If the whole part comes out a few hundredths of a millimeter short, up to 0.1 mm, the first layer has been squashed (Z offset too low): the following layers are at their proper height, but the whole part is short by that amount. If Z is always short by the same amount, suspect the Z offset first and shrinkage second. Shrinkage in Z exists, but in unfilled materials it is small and corrected separately ("Shrinkage (Z)" in Orca, "Shrinkage compensation Z" in PrusaSlicer).

Periodic bands up the height are a surface defect, not a size one (Wall marks: ringing, VFA and Z-banding).

When it fails

diagram
Start from where the error is, not from the setting: each location leads to a different cause and a different fix.
Symptom, cause and fix
Symptom Cause Fix
Error grows with size, same sign outside and inside, and changes with material Shrinkage Shrinkage compensation in the filament profile
Error grows with size in every material, often on one axis only Steps per millimeter, belt or pulley Correct the steps in firmware; check belt and pulley
Outside oversize and inside undersize by the same amount, at any size Flow or line width Flow test; then contour and hole compensation, "Precise wall"
Only the first 0.2–0.6 mm, wider; holes narrow at the bottom Elephant's foot Z offset if the first layer is squashed; default compensation + 0.5 × 45° chamfer
Only small round holes, 0.1–0.3 mm undersize Facets, bulge on the curve, ring shrinkage Fine export or STEP, hole compensation, polyholes, model larger
Oval hole (X differs from Y); a fit that goes together only one way round Belt or pulley on one axis Tension the belt, tighten the pulley grub screw
The diagonals of a square differ XY skew Square the frame, equalize the belts, correct skew in firmware
Height off by less than a layer, or the top face at the wrong height Rounding to whole layers, low Z offset Heights as multiples of layer height, "Precise Z height", Z offset
Outside dimensions oversize on textured walls Fuzzy skin or seam Measure away from them; not a fault
Different on every print Repeatability or drift Accuracy, precision and repeatability, When your numbers drift

How to test it

Print the two-size test, measure, and change a single setting before you reprint it the same way: same orientation, same material. Work in this order: flow, shrinkage, XY compensations, elephant's foot. Whatever is left inside your machine's band is handled with clearances in the design, not by retuning the slicer for every part. The full procedure, print by print, is in Dimensional calibration.

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?