kapy academy

PLA and its variants

17 min readUpdated Nov 2026

Look at the shelf in any filament shop: Basic, Matte, Silk, high-speed, PLA+, Tough+, HT, plus wood, marble and glitter. All are built on the same polymer. What differs is the additive, and the additive moves the finish, the strength between layers, how hard a knock the part survives and the temperature at which it gives way, sometimes for the worse. For anything that lives indoors, below about 40 °C, with no knocks and no permanent load, plain PLA, or matt if looks matter, is the right choice.

Plain PLA: what it gives you and why

PLA is easy to print for two physical reasons. It melts at a low temperature (nozzle at 190–230 °C; 215 °C is a good starting point). And it shrinks little as it cools, around 0.2–0.5 %, so little stress builds up between the hot layer and the cold one below, and the part barely warps. It needs no enclosure. The bed runs at 35–65 °C, usually 55–60 °C; Bambu Lab's datasheets ask for 35–45 °C on their plates. Low shrinkage is not zero shrinkage: the part still comes off with a small dimensional error. Fiber-filled grades are more stable still along the bead.

It wants the part-cooling fan at 100 % because its glass transition temperature is low: about 60 °C on the datasheet for Bambu's PLA Basic. A freshly laid bead has to drop below that temperature quickly, or overhangs and small details droop. The same fan is why PLA gives clean overhangs up to 50–60° from vertical on a modern machine, and bridges better than PETG or ABS. There is a cost: the layer below is colder by the time the next one welds to it. On a functional part loaded in Z, turning the fan down and the nozzle up improves layer bonding, at the expense of overhangs. The mechanism is in Layer adhesion and anisotropy.

It is stiff. Bambu's datasheet puts its flexural modulus at about 2.75 GPa in XY, the highest of the unfilled everyday filaments: a PLA template flexes less than the same template in PETG. Tensile strength is 35 MPa in XY and 31 MPa in Z, 89 % of the XY figure. On the datasheet's specimens, then, the layers bond well. The weakness is in how it breaks.

Elongation at break drops from 12 % in XY to 7.5 % in Z, so when it fails between layers, it fails all at once. In a knock or a snap fit it cracks instead of deforming: it tolerates around 2 % strain for a snap fit assembled once, and 1–1.5 % for a catch that opens and closes again and again. That is what "brittle" means in practice, and Print-friendly snap fits turns it into dimensions.

It absorbs little water, about 0.4 % at equilibrium at 55 % relative humidity according to Bambu's datasheets, and absorbs it slowly. Drying it at 45–55 °C for 8 h is a good idea, not a requirement; times and storage are in Drying and storing filament. Chemically, the datasheet rates it resistant to most oils and greases, but not to acids, alkalis or some solvents. The rest is in Heat, cold, sunlight and chemicals.

The variants, one by one

Every variant is base PLA plus an additive. Read each one in three steps: what was added, what changes at the nozzle and what changes in the part. To keep the comparison fair, the table uses one manufacturer's datasheets, Bambu's, with the same test methods: ISO 527 (tensile), ISO 179 (impact) and ISO 75 (HDT). The same variant from another brand will have different numbers, and the label does not tell you which. How to read these sheets is covered in Reading a material datasheet.

PLA variants from one manufacturer (Bambu Lab datasheets, November 2026)
Property Basic Matte Silk Dual Color Tough (discontinued) Tough+
Nozzle (°C) 190–230 190–230 210–240 — 220–250
Maximum speed per datasheet (mm/s) < 300 < 300 < 250 — < 300
Melt flow index, 210 °C / 2.16 kg (g/10 min) 42.4 — 20.5 — 18.0
Density (g/cm³) 1.26 1.31 1.32 — 1.21
Tensile XY / Z (MPa) 35 / 31 32 / 25 27 / 18 44 / 39 34.9 / 20.9
Z as a share of XY 89 % 78 % 67 % 89 % 60 %
Elongation at break XY / Z (%) 12 / 7.5 32.8 / 4.8 3.5 / 1.7 8.2 / 5.6 9.4 / 9.3
Unnotched impact XY (kJ/m²) 26.6 19.2 — — 80.6
Notched impact XY (kJ/m²) 7.9 6.3 — — 72.3
Unnotched impact Z (kJ/m²) 13.8 6.6 4.6 — 25.9
Flexural modulus (MPa) 2750 — — — 2140
HDT at 0.45 MPa (°C) 57 58 53 55 61

A dash means the datasheet gives no figure. The sheets are PLA Basic V3.0 for tensile and V2.0 for the rest, Matte V2.0, Silk Dual Color V3.0, Tough V1.0 and Tough+ V3.0. PLA Tough is no longer made; it stays in the table because it shows the other way to "improve" PLA. The Tough+ specimens were printed at 245 °C and annealed at 50 °C for 8 h before testing: the same test method, but not the as-printed condition of the others.

Tensile strength (MPa)XY, along the beadZ, between layersBasic353189 %Matte322578 %Silk271867 %Tough443989 %Tough+352160 %01020304050HDT at 0.45 MPa (°C)Basic57Matte58Silk53Tough55Tough+61PLA-HT as printed~70PLA-HT annealed~10530405060708090100110Loaded design limit, ~40 °CDashboard in summer, 70–100 °CBambu Lab (variants) and Polymaker (HT-PLA), ISO 527 / ISO 75
The additive moves the properties. The finish variants lose most between layers; Tough+ gains impact, not temperature. Only annealed PLA-HT gets close to dashboard temperatures, and under load it is not enough.

Matt

Matt PLA carries a mineral filler that manufacturers rarely specify. The particles roughen the surface at the micron scale and scatter light in every direction, so layer lines and small defects all but vanish. You can see the filler in the density: 1.31 g/cm³ against 1.26 for Basic, so a kilo gives you fewer meters.

The layer weld pays the price: the particles take up room at the interface that would otherwise be polymer. Bambu's PLA Matte gives 32 MPa in XY but 25 in Z, 78 %. Its elongation is high along the bead (32.8 %) and drops to 4.8 % between layers, and notched impact falls to 6.3 kJ/m² against 7.9 for Basic. HDT does not change: 58 °C. Use it for parts that only have to look good: models, organizers, enclosures. Avoid it for fine features loaded between layers. If you iron the top layers, matt can show the nozzle's tracks.

Silk

Silk is PLA blended with additives that leave the bead smooth and glossy; Bambu does not say which. You notice it at the nozzle: the melt flows less readily. The melt flow index of Silk Dual Color is 20.5 g/10 min against 42.4 for Basic, measured under the same conditions. To melt the same volume it needs more heat or less speed, and the datasheet reflects that: 210–240 °C and under 250 mm/s, against 190–230 °C and 300 mm/s for Basic. The shine also depends on how you print it: hotter and slower shines more. The bead tends to swell as it leaves the nozzle, so you usually have to lower the flow ratio. A silk spool deserves its own calibration.

Its mechanical cost is the largest in the family and the most often ignored. On its datasheet, Bambu's PLA Silk Dual Color gives 27 MPa in XY and 18 in Z, 67 %. It stretches 3.5 % in XY and 1.7 % in Z before breaking, its impact strength in Z is 4.6 kJ/m², a third of Basic's, and flexural strength drops from 66 MPa in XY to 21 in Z. HDT is 53 °C on that sheet; the single-color Silk+ that Bambu sells today claims 60 °C, so silk does not have to cost you heat resistance. It does cost you ductility: Silk+ stops at 2.8 % elongation. The rule: never use silk for a clip, a hinge or a thread, or for anything loaded between layers. The color effect of co-extruded dual- and tri-color silk is covered in Decorative filaments.

Plain PLALayer weldMattDiffuse reflectionMineral fillerSilkSpecular reflectionDie swell
Matt PLA's filler scatters light and takes up room in the weld; silk reflects in one direction, swells on leaving the nozzle and welds through a thinner neck. That is why both lose more in Z than in XY.

High-speed

It is sold as "Hyper", "Rapid", "HS" or "HF", and Bambu's own PLA Basic is advertised for 250–300 mm/s. It is a lower-viscosity grade, with a higher melt flow index, that flows more readily at the same nozzle temperature, so the hotend reaches more mm³/s before it under-extrudes.

What limits speed is not mm/s but volumetric flow: speed × line width × layer height. The "600 mm/s" printed on some spools works out at 600 × 0.45 × 0.20 = 54 mm³/s, two to three and a half times what a standard hotend really melts with PLA (15–25 mm³/s). Bambu Studio caps its PLA Basic at 21 mm³/s on the X1 and P1, which at 0.45 × 0.20 mm is 233 mm/s; Prusa caps Prusament PLA at 15 mm³/s with the standard nozzle and 24 with the high-flow one. Your hotend sets the ceiling, and the filament only lets you get closer to it. The physics is in Volumetric flow sets the speed, and how to measure your own ceiling in Flow ratio and max flow tests. The cost: a runnier melt strings more and droops a little more if cooling cannot keep up. At moderate speed, a high-speed PLA prints like a normal one.

PLA+, Pro and Tough

No standard sits behind these names. Each manufacturer uses them for its own modified PLA, nearly always with impact modifiers, and from some brands it is barely distinguishable from plain PLA on the datasheet. Bambu's range shows both ways to "improve" PLA. The old PLA Tough raised tensile strength to 44 MPa in XY and 39 in Z, with a slightly lower HDT: 55 °C. Tough+, which replaced it in 2025, goes for toughness: it triples unnotched impact in XY (80.6 against 26.6 kJ/m²) and nearly doubles it in Z (25.9 against 13.8). Notched, the figure that counts for a part with sharp corners, it goes from 7.9 to 72.3.

The price is stiffness and layer strength. Its flexural modulus drops to 2140 MPa, 22 % below Basic, and tensile strength in Z only reaches 20.9 MPa, 60 % of its XY value against 89 % for Basic. It gains little in temperature: an HDT of 61 °C. It is a material for parts that take knocks, not for loads carried between layers. What "tough" actually measures is explained in Stiffness, strength and toughness.

Tough PLAs want a nozzle temperature at the top of the range, and Tough+ goes beyond it: 220–250 °C. They stick harder to supports, and Bambu recommends a support interface in a different material. Being softer, they creep more under sustained load. Brand A's PLA+ tells you nothing about brand B's: read its datasheet or print your own test specimen.

PLA-HT

A nucleated grade that crystallizes quickly. After annealing, its HDT rises from about 70 °C as printed to about 105 °C: Polymaker's HT-PLA goes from 69.9 to 106.5 °C. It prints at 200–230 °C with the bed at 50–60 °C, and annealing adds 1–5 % shrinkage in XY. Without an oven it is only a slightly better PLA. The full process is in Annealing and strengthening.

Fiber and other fillers

Carbon- and glass-fiber PLA, wood, marble, glitter and glow-in-the-dark PLA are all PLA with a filler. They print at 210–240 °C and nearly all are abrasive: they need a hardened nozzle. They are covered in Carbon and glass fiber filaments and Decorative filaments; foaming PLA (LW-PLA) in Functional specialty filaments.

Settings per variant

Only the differences from plain PLA are listed here. The baseline: 215 °C, part-cooling fan at 100 %, smooth PEI, textured PEI or a cool plate, and glue only as a release agent on the cool plate.

  • Silk: 10–15 °C more at the nozzle, slower outer walls and a lower flow ratio. If it comes out dull, raise the temperature or lower the speed before touching anything else.
  • Matt: the same temperatures as Basic. It hides the seam better than any other variant.
  • High-speed: only makes a difference once you exceed the standard grade's maximum flow. Below that, it prints like plain PLA.
  • Tough and PLA+: the top of the nozzle range (220–250 °C for Tough+) and a support interface in a different material, or a larger Z gap. If supports end up welded to the part, this is the cause. The Tough+ datasheet also recommends glue on the bed.

A matt, a silk and a Basic from the same brand have three different flow ratios and three different maximum flows: one profile per variant. Changing variant also changes how your fits come out; Real printed clearances explains how to check.

In an enclosed printer, open the door or lid for PLA once the bed is above about 45 °C (Enclosures and heated chambers): with everything closed, heat climbs the hotend and softens the filament before the melt zone. That is heat creep, and it ends in a clog (Extrusion problems).

Where PLA falls short

Heat

Plain PLA's HDT at 0.45 MPa is 57 °C (52–60 °C depending on the source); matt gives 58, silk between 53 and 60 and Tough+ 61. No variant raises it noticeably except annealed PLA-HT. Under load, an amorphous plastic such as PLA works up to about 15–20 °C below its HDT at 0.45 MPa: PLA, about 40 °C (Heat, cold, sunlight and chemicals). Bambu advises against PLA in environments at or above about 50 °C. Inside a car, never PLA: in summer, the dashboard in the sun reaches 70–100 °C. Loaded and in the sun, not even annealed PLA-HT will do, since under load it tops out at about 85 °C; that needs a fiber-filled compound (PA-CF, PET-CF or PPA-CF). Unloaded or in the shade, in the console or the glovebox, annealed PLA-HT works, as do ASA and PC (Choosing a filament).

Sustained load

Under a sustained load, PLA is only comfortable below about 30 °C and its limit under load is around 40 °C (Creep and fatigue). A shelf bracket that holds today next to a sunny window may be sagging in a few months.

Repeated flexing and impact

With 1–1.5 % allowable strain in repeated use, clips, living hinges, latches and enclosures that get dropped belong to PETG or PCTG, the polyamides or polypropylene. Tough+ widens the margin against knocks, not against fatigue. Living hinges and flexures explains why PLA will not do for hinges.

Outdoors

In the sun, heat and ultraviolet light soften and degrade it within a few seasons. The outdoor material is ASA.

Three myths to drop:

  • "It is biodegradable." Only under industrial composting conditions, not in a drawer or a field. More in Printing with less waste.
  • "It is food-safe because it comes from corn." That depends on the printed part, the colorant and the nozzle, not on where the polymer came from. See Printing for food contact.
  • "It emits nothing." It emits the least of the common filaments, but not zero: about 2 × 10¹⁰ ultrafine particles per minute against about 2 × 10¹¹ for ABS in the first study to measure them. Details in Emissions and ventilation.
diagram
Start from what the part has to withstand. Looks and the odd knock indoors stay in PLA; heat only keeps you there with annealed PLA-HT, and sunlight, repeated flexing and permanent load take you out of the family.

When to change material, and to what

When it fails

Symptom, cause and fix
Symptom Cause Fix
Silk comes out dull Nozzle too cold or outer wall too fast Raise it 10–15 °C or slow down before touching anything else
A silk or matt clip, hinge or thread breaks between layers Weak layer bond: 67–78 % of XY PLA Basic or Tough+, or move to PETG
Supports end up welded to a Tough+ or PLA+ part Tough PLAs stick harder to their supports A support interface in another material, or a larger Z gap
Under-extrusion at high speed Flow above the hotend's ceiling, not the filament's Drop to the measured maximum flow (Flow ratio and max flow tests)
Clogs on long prints in an enclosed CoreXY Heat creep: door shut with the bed above about 45 °C Open the door or the lid
Stringing Damp spool or nozzle too hot Dry it and lower the temperature (Stringing and blobs)
A part has sagged in the sun or in the car Above about 40 °C under load ASA or PC; in a car, depending on the load (Choosing a filament)

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?