kapy academy

Reading a material datasheet

17 min readUpdated Nov 2026

You have two spools in your basket and every product page links a PDF full of numbers, of which you need only the ones that decide your part. Bambu Lab's V3.0 datasheet for PLA Basic gives 35 MPa of tensile strength along the beads (XY) and 31 MPa across the layers (Z); Polymaker's for PolyLite PLA gives 52.3 and 40.5. Same plastic, a 50 % difference. And neither is your part's number: each comes from a solid, dry test bar printed and tested in the manufacturer's own lab.

How the test bar was made

Bambu Lab, Polymaker and Prusament test printed bars and separate XY from Z. Injection-molded bars are what the resin datasheet tests, the one the maker of the pellets publishes, and some small filament brands still copy those values. If the sheet does not separate XY from Z and does not say what settings the bar was printed with, assume it is resin data: your printed part will come out well below it.

Printed does not mean realistic. These are the conditions the datasheets declare:

  • Bambu PLA Basic (V2.0 datasheet, the one with 39 and 35 MPa; V3.0 changed the values): nozzle at 220 °C, 200 mm/s, 100 % infill, bars dried and conditioned for 8 h at 55 °C before testing. The sheet calls this "annealing", but 55 °C is below PLA's glass transition temperature (Tg), around 60 °C: it is drying, not annealing.
  • Polymaker PolyLite PLA: 230 °C, 2 walls, 3 top and bottom layers, 100 % infill, fan on.
  • Prusament PLA: a Prusa MK3, 0.20 mm layers, 2 walls, 100 % rectilinear infill at 200 mm/s.

Your part, on the other hand, has 15 % infill, a seam, long layer times on the big sections and a filament that has been picking up moisture for weeks.

The standard fixes the bar's shape and the test speed. European datasheets cite ISO 527 (tensile), ISO 178 (flexural), ISO 179 (Charpy impact), ISO 75 (HDT), ISO 306 (Vicat), ISO 1133 (melt flow index) and ISO 1183 (density). American ones cite ASTM D638, D790, D256 (Izod) and D648. In tension and bending, ISO and ASTM give similar but not identical values. For impact there is no conversion: ASTM D256 Izod is in J/m, while ISO 179 Charpy (like ISO 180 Izod) is in kJ/m². The bar, the supports and the notch are all different.

The most serious trap is on the sheet itself: orientation. XY is the bar lying flat, with the beads running along it. Z is the bar standing up: when you pull on it, you pull every layer joint apart. Prusament's datasheet labels its second column "vertical xz": that is a bar printed on its edge, with the beads still running along it, so it is not a Z value. That is why it does not drop the way a Z value would: it gives 59 MPa, even more than the 51 of the flat bar. Prusament measures layer bonding separately ("interlayer adhesion"): 17 ± 3 MPa. Before you read a column as Z, check the drawing or the axis label.

The same tensile bar printed three ways on a bed: flat (XY), on edge (XZ, the column some datasheets call 'vertical') and upright (Z). They print together layer by layer and are then pulled with the same force: the first two hold, with their beads along the length; the upright one parts cleanly between two layers. Prusament PLA values: 51, 59 and 17 MPa.
Only the upright bar is tested across the layers; the edgewise one, which some datasheets call 'vertical', is still tested along the beads. Prusament PLA datasheet values; layers drawn 1 mm thick so they show.

The ± is the scatter across a few bars from one batch tested on the same day (35 ± 3 MPa, for example). It says nothing about variation between spools, colors or printers. Datasheets also get revised: Bambu Lab's PLA Basic sheet gave 39 MPa in XY and 35 in Z in V2.0, and 35 and 31 in V3.0. When you note down a number, note the version and date too.

What each number measures

The rows of a filament datasheet
Property Standard · unit What it tells you The trap
Density ISO 1183 · g/cm³ Grams and cost per part Compare price per cm³, not per kg
Melt flow index (MFI/MFR) ISO 1133 · g/10 min How freely the melt flows Only comparable at the same temperature and weight
Glass transition temperature (Tg) ISO 11357-2 (DSC) · °C Ceiling for amorphous plastics and printed PLA Not a ceiling for semi-crystalline ones
Vicat softening temperature ISO 306 · °C When the surface softens Not a service temperature
Heat deflection temperature (HDT) ISO 75 · °C Temperature at which a loaded bar gives way 0.45 MPa and 1.8 MPa do not compare
Tensile modulus ISO 527 · MPa or GPa Stiffness when stretched Do not mix it with the flexural one
Flexural modulus ISO 178 · MPa or GPa Stiffness when bent The one a bending part uses
Tensile strength ISO 527 · MPa Stress at which it yields or breaks Check whether it is yield or break
Flexural strength ISO 178 · MPa Peak stress on the outer face Never for sizing
Elongation at break ISO 527 · % How far it stretches before breaking Check the Z value too
Charpy impact strength ISO 179 · kJ/m² Energy absorbed by a blow Notched and unnotched; only within one brand
Water absorption % · conditions How much water it takes up Decisive for nylon
Hardness Shore A/D How soft it is Only matters for TPU and flexibles

Density changes what you pay: PLA sits around 1.24–1.26 g/cm³ and ABS and ASA at 1.05, so a kilo of ABS gives you 18–20 % more volume than a kilo of PLA. Melt flow index only compares at the same temperature and weight: Bambu Lab's PLA Basic gives 42.4 g/10 min (V2.0 datasheet) and Prusament PLA 9–11, both at 210 °C and 2.16 kg. A high index helps the plastic melt and extrude faster, although flow is limited mainly by the hotend. It does not measure strength: at most it hints at shorter chains, which tend to give a little less toughness, and it never ranks two brands.

Tg is the ceiling for amorphous plastics (PETG, ABS, ASA, PC) and for PLA as it comes off the printer, which is almost amorphous. It is not a ceiling for semi-crystalline ones (nylon, PP, PEEK, fiber-filled PA and PPA): their crystals keep them stiff well above Tg. That is why PAHT-CF's HDT (194 °C) sits so far above its Tg. Check the method too: a Tg measured by DMA usually comes out higher than one by DSC. The Vicat temperature is the point at which a loaded needle (10 N in method A, 50 N in method B) sinks 1 mm; for PLA it lands close to the HDT (57 and 57 °C on Bambu Lab's V2.0 sheet, 63 and 60 °C on PolyLite's).

HDT is the temperature at which a bar under a fixed bending stress deflects by the amount the standard sets. Method B loads it to 0.45 MPa and method A to 1.8 MPa; this book quotes the 0.45 MPa figure unless it says otherwise. The gap between the two tells you something as well. In PLA it is tiny (Bambu 57/54 °C, Prusament 55/55 °C) because PLA loses its stiffness all at once when it reaches Tg. In semi-crystalline composites it is wide (PAHT-CF 194/170 °C), which is why the service rule depends on the structure: under load, design 15–20 °C below the HDT at 0.45 MPa if the plastic is amorphous, and 15–20 °C below the HDT at 1.8 MPa if it is semi-crystalline, with or without fiber (Heat, cold, sunlight and chemicals).

The two moduli come from different tests. In an isotropic material they would match; in a printed bar they diverge because of test speed, support and the structure of walls and voids. On filament datasheets they bear no fixed relationship: Bambu Lab's V2.0 sheet for ABS gives 3.8 GPa in tension and 1.9 GPa in bending. A bracket, an arm or a lid works in bending, so use the flexural modulus, and never mix one brand's tensile modulus with another's flexural one.

For tensile strength, check which value you are given. Yield strength (Prusament gives "tensile yield strength") is the maximum before the bar starts to neck; strength at break is the stress at which it snaps. For a ductile material, the useful design number is yield. Flexural strength always comes out higher than tensile strength for the same material (76 against 39 MPa on the V2.0 PLA Basic sheet). Only a thin band on the outer face reaches the peak, and the bending formula assumes the material stays elastic to the end, so it overstates the stress once the plastic has yielded. Never size a part with it.

Elongation at break is the handiest indicator of toughness. Read the Z value too, because it drops proportionally more than strength (PLA from 12 to 7.5 %, PETG from 9.5 to 5.2 %): that is why a part that breaks between layers gives no warning.

Charpy impact strength is three or more times higher without the notch (V2.0 PLA Basic sheet: 26.6 kJ/m² unnotched, 7.9 notched). Measured on printed bars, it ranks materials badly: Bambu Lab's datasheets put PC at 7.5 kJ/m² in XY, below PETG's 21.6, exactly the opposite of what happens when you drop a PC part. PC is very notch-sensitive, and the joints between beads in a printed bar act as notches. Compare impact only within one manufacturer's datasheets, with the same notch and the same direction; if you cannot, trust elongation instead.

Water absorption matters for nylon, and the sheet usually gives its values dry (more on that below, under what the datasheet leaves out). Shore hardness is the number that rules in TPU and flexible filaments; for a rigid plastic it is only a catalog figure. PC and engineering-material datasheets add two more rows: UL 94 flammability (V-0, V-2, HB), which only holds at the stated thickness and, if it comes from the resin, does not certify your printed part; and the coefficient of linear thermal expansion (CLTE), which matters when the part mates with metal.

Compare in relative terms, within one brand

Put three PLA datasheets side by side:

Three PLA datasheets, November 2026
Datasheet Tensile XY Tensile Z Elongation XY HDT 0.45 MPa
Bambu Lab PLA Basic V3.0 35 MPa 31 MPa 12 % 57 °C
Polymaker PolyLite PLA 52.3 MPa 40.5 MPa 6.3 % (Z 1.8 %) 60 °C
Prusament PLA V1.1 51 MPa (yield) 17 MPa (interlayer) not given 55 °C

Same polymer, and the ranking changes from row to row. PolyLite is the strongest and the one that stretches least; Bambu Lab's is weaker but stretches almost twice as far. Behind that are the formulation (PLA grade, additives, impact modifiers), the bar's settings (temperature, speed, walls, infill direction), conditioning and test speed. None of it shows in the number.

Bambu Lab PLA Basic V3.0Polymaker PolyLite PLAPrusament PLA V1.1Tensile strength (MPa)0204060353152.340.55117interlayerXYZElongation at break XY (%)051015126.3not givenHDT at 0.45 MPa (°C)405060576055Manufacturers' datasheets, checked November 2026
Three PLA datasheets and no clear winner: the ranking changes from row to row. Numbers from different labs cannot rank brands.

The rule: compare materials using datasheets from the same manufacturer. The lab, printer, bar and method are the same, and then the ratios between materials are reliable: PC's HDT sits about 45 °C above PETG's, and PPS-CF keeps far less of its strength in Z than PC does (28 % against 90 %). Between manufacturers, treat differences under 20–30 % as noise; between two brands, let a coupon of your own decide. Use the datasheet to choose and rank, and size the part with your own coupon printed in the part's orientation (Test coupons). The full table, read this way, is in Filament comparison table.

The Z column is the useful one

On a modern datasheet, the ratio between Z and XY tells you how forgiving the material is of a bad orientation. Z/XY on Bambu Lab's datasheets: PLA 89 %, PETG 69 %, ASA 67 %, PC 90 %, PAHT-CF 51 %, PPS-CF 28 %, TPU 85A 88 %.

Those are ideal bars. For design, assume the part is half as strong in Z as in XY, or 30 % if the material is fiber-filled, and orient it so the main load runs along the beads (Layer adhesion and anisotropy). In a real part, long layer times, too much fan, printing ABS, ASA, PC or nylon without an enclosure, or damp filament bring it down to 20–40 %.

Fiber-filled grades come out best in XY and worst in Z. The fiber lies along the bead and stiffens it, but it does not cross the weld between layers: a PPS-CF with 87 MPa in XY holds 24 MPa across the layers. If the sheet gives no Z value, do not assume it is close to XY: use 50 or 30 %.

What the datasheet leaves out

  • Load over time. Every number comes from a test lasting minutes. Under constant load plastic deforms over time (PLA and PETG noticeably, even at room temperature), and repeated loads open up the layer joints well below the breaking load. Molding-grade datasheets sometimes give a creep modulus (ISO 899-1); almost no filament datasheet carries creep or fatigue data: Creep and fatigue.
  • Temperature. Every mechanical row is measured at about 23 °C. Stiffness falls steadily as the part approaches its HDT; a PLA bracket in a room at 40 °C is already softer than the sheet says: Heat, cold, sunlight and chemicals.
  • Sunlight and chemicals. At best, a qualitative row. Bambu Lab's PLA Basic sheet says it does not resist acids, alkalis or some solvents, and does resist most oils and greases. It gives no hours of UV exposure and no solvent concentrations: Heat, cold, sunlight and chemicals.
  • Shrinkage. It rarely appears, and when it does it is a molding figure. Yet shrinkage is what drives your settings: Shrinkage and dimensional stability.
  • Moisture. Nylon values are usually dry, straight out of the dryer. Conditioned to ambient humidity, nylon is clearly less stiff and more ductile: Nylons and polyamides.
  • Food contact and safety. The technical datasheet (TDS) is not the safety data sheet (SDS), and neither is a declaration of compliance for food contact. "Food safe" on a product page is not a datasheet row: Printing for food contact. Fumes and particles are covered in Emissions and ventilation.
  • Color and batch. The bars are one color from one batch. Heavily pigmented, silk, glow-in-the-dark or filled versions (fiber, metal, wood) are different products, with their own datasheet and almost always more brittle.

Let the part pick the number

Almost every part has one requirement that governs it, and that requirement points to a single row. Read that row and use the rest as tie-breakers.

  • It must not bend: flexural modulus, in XY, or in Z if it bends across the layers.
  • It must not break under a point load: tensile strength, along the beads or in Z depending on orientation.
  • It must survive a knock or a drop: elongation at break; impact only within one manufacturer's datasheets.
  • It must take heat: HDT minus 15–20 °C, at 0.45 MPa if amorphous and at 1.8 MPa if semi-crystalline.
  • It must carry a load for months, live outdoors, touch food or hold a fit: not on the datasheet. Go to the article that covers it.
diagram
The requirement that governs the part picks one row of the datasheet. Four other common requirements appear on no row at all: each has its own article.

Then size it. The datasheet number goes into a hand calculation together with the orientation factor and a safety factor (Estimating whether a part will hold), and a printed coupon has the final say (Test coupons).

When it fails

Symptom, cause and fix
Symptom Cause Fix
You chose the PLA with the highest tensile strength and it broke on the first drop Strength is not toughness; that sheet gave 6 % elongation Read elongation; impact only within one brand
You compared two brands' HDT and the one that "took more heat" gave way first One figure was at 1.8 MPa, or it was a Vicat temperature Check load and method; compare at the same load
You read Prusament's "vertical" column as Z and printed the bracket upright "Vertical xz" is edgewise: the beads still run along the bar Use the interlayer value or 50 % of XY
You sized the part with flexural strength and it broke at half the load The bending test overstates strength Use tensile strength with the orientation factor
The nylon part bent far more than the modulus predicted The sheet was dry and your part has taken up water Use conditioned values or derate the modulus; condition the coupon the way the part will live
You used a molded-bar value from the resin datasheet and the print came out much weaker Sheet without XY or Z: resin data Find a sheet with printed XY and Z values, or test

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?