The first layer is the only one printed onto something that is not plastic: the bead grips the plate only because the nozzle presses it down while it is still soft. If it fails, the part comes loose, a corner lifts or the base prints wide. With automatic probing, leave the profile's first-layer settings alone (0.20 × 0.50 mm with a 0.4 nozzle, 30 to 50 mm/s, fan off), wash the plate with water and washing-up liquid, and watch the first layer while it prints. If it fails, check in this order: cleanliness, Z offset, bed temperature, then the rest.

Why the first bead sticks

Plastic does not weld to PEI or glass the way it welds to itself. It holds by contact area, and that contact only forms while the plastic is molten: it works into the texture of a rough plate or wets a smooth, clean one. After that, the heated bed keeps the base near its glass transition temperature so shrinkage does not tear it off. The more of the bead touches the plate, the better it holds: a round bead rests on a narrow strip; a squished one rests on its full width.

contactplatenozzleNozzle too highcontact0.50 mm0.20 mmRightnominal outlineelephant's footNozzle too low
The same bead at three Z offsets. Nozzle too high: the bead touches the plate along a narrow strip. Right: across its full width. Too low: the nozzle shoves the plastic sideways and out past the outline.

The slicer sets the squish. The nozzle does not sit "less than a layer height" above the plate, as people often say: it sits at 0.20 mm, the first-layer height. What does the squishing is the width: with a 0.4 nozzle, Bambu Studio and PrusaSlicer ask for a 0.50 mm line width. That is a width-to-height ratio of 2.5, against 2.25 for an ordinary 0.45 × 0.20 bead. The plastic has nowhere to go but sideways and down into the texture. A correct Z offset does the rest.

First-layer height and width, and why a thinner one is a bad idea, are in Layer height and line width: with a 0.4 nozzle, do not go below about 0.15 mm; with a 0.6, the first layer is 0.30 × 0.65–0.68 mm.

The window is narrow. Moving the Z offset by 0.02–0.05 mm is enough to go from round beads to correct ones, or from correct to over-squished. That is 0.05 mm: a quarter of a 0.20 layer. This is why the plate has to sit at the same distance from the nozzle everywhere, and why the Z offset is the first setting you check after cleaning the plate.

Z offset and mesh: what puts the nozzle at the right height

The printer probes a grid of points and corrects Z on the fly so the nozzle follows the shape of the plate. The mesh corrects shape (a tilt, a dip, a bulge in the middle), not the absolute distance between nozzle and plate. That distance is the Z offset.

Who sets it depends on how the machine probes. On printers that probe with the nozzle itself, through a load cell or strain gauge, the reference is the nozzle touching the plate, and the Z offset is calibrated automatically on every print. As of late 2026, that includes modern bedslingers such as the Bambu A1 or the Prusa MK4S, and enclosed CoreXY machines such as the Prusa CORE One. Prusa says manual first-layer calibration is unnecessary on its load-cell printers; "Live Adjust Z" is there for fine-tuning. On machines with a separate probe (inductive, BLTouch-style or eddy current) there is a fixed distance between probe and nozzle tip: you enter the Z offset yourself, and you have to set it again every time you change the nozzle. The exception is eddy-current probes with a contact mode, which set the Z offset by touching the plate with the nozzle.

Probing with the nozzle has one weak point: the nozzle. A blob of plastic stuck to the tip touches the plate before the metal does, the firmware thinks the plate is higher, and the first layer prints high. That is why these machines wipe the tip and probe with the nozzle warm, not hot enough to ooze. If you see round beads right after a clog or a filament change, clean the tip hot with a brass brush and probe again.

Even with an automatic Z offset, you will sometimes need to adjust it:

  • When you change plates: on a textured plate the nozzle touches the peaks and the plastic also has the valleys to flow into, so the same Z offset squishes differently on smooth and textured.
  • When you change material: PETG usually runs with the nozzle a little further from the plate, so it does not stick too hard or get dragged by the nozzle. The amount varies with the material; do not treat it as a fixed rule.
  • On a worn or dented plate.

Adjust in steps of 0.01–0.02 mm while the first layer prints: "Live Adjust Z" on a Prusa, or baby-stepping in Klipper or Marlin. If your printer cannot adjust it live, use the "Z offset" field in OrcaSlicer's printer settings and slice again. The sign changes from one interface to the next, so think "nozzle closer to the plate" or "further away", not up or down a number. Judge the result after a full pass over a large area, not on the skirt: it is a single line and proves nothing. Save the value: on a Prusa it is stored with the plate profile selected on the printer; in Klipper, with Z_OFFSET_APPLY_PROBE (or Z_OFFSET_APPLY_ENDSTOP) and SAVE_CONFIG, or it is lost at power-off.

The mesh can fail too. A mesh probed on a cold bed is wrong on a hot one, because the bed and the gantry expand: probe the bed hot, after a few minutes of preheating (Bed probing and Z offset). Probe the area the part covers (adaptive mesh) or the whole plate, but do not reuse a mesh after moving the printer or changing the plate.

On a legacy bedslinger with manual leveling, you level with a sheet of paper. An 80 g/m² sheet is about 0.1 mm thick: it gets you close, and live adjustment on a printed pattern does the rest.

Speed, temperature and fan on the first layer

First layer: starting values (0.4 nozzle)
Setting Value Why
Height × width 0.20 × 0.50 mm A 2.5 ratio: the bead is squished into the plate
Speed 30–50 mm/s (rest of the part: 150–500 depending on the machine) The bead needs contact time while hot
Acceleration ≈500 mm/s² (Prusa) Sharp changes drag a bead that has not gripped yet
Nozzle The filament's temperature or 5–10 °C above Hotter plastic works further into the texture
Bed, PLA 55–60 °C (35–65) Keeps the base soft and in contact
Bed, PETG 70 °C (60–80) Bonds too hard to smooth PEI: textured plate or glue as a release agent
Bed, ABS/ASA 90–110 °C They shrink a lot: without an enclosure, the corners peel
Fan Off Air cools the bead before it spreads

The bead has to stay in contact with the plate while it is still hot, and fast changes of direction drag a freshly laid bead before it grips. Going below about 20 mm/s rarely helps on a clean, well-set plate, and it costs time when the first layer covers the whole plate.

Profiles print the first layer at the filament's normal temperature or 5–10 °C above it: hotter plastic flows further into the texture and takes a little longer to set. Do not use temperature to cover for a bad Z offset.

The bed keeps the base of the part near or above its glass transition temperature, soft enough to stay in contact, and it eases the pull of shrinkage at the corners. Too hot fails too: PLA on a bed above about 65 °C stays soft, the first layers give under the weight of those above, and the elephant's foot grows. In an enclosed printer, open the door for PLA, PVA or TPU once the bed is above about 45 °C, and for PETG above about 70 °C (Enclosures and heated chambers); with the door shut, the hotend jams from heat creep. Surfaces, glues and release agents per material are in Bed prep for each material.

Profiles switch the fan off for the first layer, and sometimes for the next two or three; in Bambu Studio the field is "No cooling for the first". Air cools the bead below its glass transition temperature before it has spread over the plate. A fan that starts too early is a common cause of lifted corners on small parts. Full cooling curves are in Speed and cooling.

Drafts do what the fan does, but from one side only: an open window or air conditioning blowing on a bedslinger. On an enclosed CoreXY, the enclosure takes care of it.

Reading a first layer

The same first layer, four 0.50 mm lines at a 0.45 pitch, printed at three Z offsets and seen from the front on the plate as the nozzle lays it: at 0.40 mm the beads fall round, touch the plate along a line and leave gaps; at 0.20 mm flat ribbons fuse and rest across their full width; at 0.08 mm the nozzle shoves the plastic up into ridges and the first line spills past the outline as elephant's foot
The same first layer at three Z offsets, seen from the front: each line's section tells you where the nozzle was. Too high, round loose beads; at the right height, one continuous sheet; too low, ridges and elephant's foot. Lines drawn ×100; the offsets are examples.
  • Nozzle too high: round, separate beads with dark gaps or the plate showing between them; ends that do not join; beads that curl or get dragged by the nozzle at corners. The square lifts off with a fingernail and falls apart into loose strands, because they never welded together. Bring the nozzle closer to the plate.
  • Right: flat ribbons fused into a single sheet where you can barely pick out individual beads; even width; smooth to the touch, with very faint ridging. The underside copies the plate texture evenly. A thin square peels off the cold plate in one piece without breaking up.
  • Nozzle too low: thin, almost translucent beads; ridges and furrows where the nozzle plows the material aside; a rough, scaly surface. The first beads may be missing or broken because there is no room for the plastic, the extruder may click, plastic builds up on the nozzle and the excess spills past the outline as elephant's foot. Move the nozzle away from the plate.

Where the defect shows tells you what to adjust:

diagram
What you see in the first layer decides what you adjust: the Z offset is only the answer when the defect is the same across the whole plate.

Flow disguises itself as Z offset. A filament profile that over-extrudes looks like a nozzle that is too low (ridges); one that under-extrudes looks like a nozzle that is too high (gaps). If the same Z offset works for one filament and not another, check that filament's flow before touching the Z offset (Flow ratio and max flow tests; the order is in What to calibrate, and in what order).

Watch the first layer before you walk away. Some machines inspect it themselves with lidar or the camera, but they only catch the big failures; your eye catches the half-millimeter one (Sensors, cameras and failure detection). A bad first layer does not fix itself higher up: stop, correct and start again.

What to check first when the part will not stick

The plate comes first because, on a machine that probes, the Z offset is usually right out of the box and what changes from one print to the next is how clean the plate is. A clean textured PEI plate holds PLA and PETG without glue at the temperatures in the table. Do not use acetone on textured PEI: it is a powder coating, and acetone attacks it. The detail per surface is in Bed prep for each material.

Do not fix warping by squishing harder. Over-squishing to hold a corner down trades a warped part for a wide base and holes that narrow at the bottom. Warping is a shrinkage force; you fight it with bed temperature, an enclosure, a brim and rounded corners on the footprint (Warping and lifting corners, Brims, rafts and mouse ears). A raft is not the cure for a badly leveled bed either: on a machine that probes, that is fixed with the mesh and the plate.

A PEI plate loses grip where it is used most. If it has stopped holding in the middle, flip it over or replace it (Bed and motion upkeep).

The price of squish: the base prints wide

The plastic a wide, squished bead displaces goes sideways, past the nominal outline, on the first layer and, with the bed hot and weight on top, on the next two or three: the bottom 0.2 to 0.6 mm of the part. That is elephant's foot. Outer contours grow, vertical holes narrow at the base, and the more you squish, the bigger the foot.

Keep the slicer's elephant's foot compensation at its default, 0.075 to 0.2 mm depending on the machine, and add a 0.5 × 45° chamfer to the edge on the bed: the compensation fixes the squish and the chamfer hides the rest. They stack (The face on the bed). Do not raise the compensation far above its default: it cuts the area that sticks. Holes that narrow at the bottom are in Why holes print small; how to measure elephant's foot, in Parts that print the wrong size.

Designing parts that stick

Contact area decides the grip. Put the largest flat face on the plate when the function allows it (Orientation and overhangs). A part resting on a few small islands or on an edge has almost nothing holding it.

Peeling starts at the corners of the footprint. Rounding those corners in plan spreads the stress along the outline. Do not confuse this with a fillet on the bottom edge, between the resting face and the walls: that fillet removes contact area and prints as an overhang stuck to the plate. A 40 × 40 mm box with a 3 mm fillet on its bottom edge has a flat face of only 34 × 34 mm, 1,156 of its 1,600 mm²; the printed first layer adds a strip under 1 mm wide where the fillet starts. That edge gets a chamfer (The face on the bed).

When it fails

On a machine with automatic probing, these are the causes, from most to least common.

The part will not stick: symptom, cause and fix
Symptom Cause Fix
Comes loose early; the beads look fine Dirty plate: finger grease Wash with warm water and washing-up liquid, dry it, and keep your fingers off the print area. Isopropyl alcohol between washes only removes some of the grease
Round beads across the whole plate Nozzle too high, or debris on its tip Clean the tip and bring the nozzle closer 0.01–0.02 mm per step
Good on one side, bad on the other Mesh, badly seated plate, dirt underneath or a bed that is not flat Clean under the plate, seat it and probe again
Bad only in patches Finger grease or a damaged plate Wash the plate; if it is worn, flip it over or replace it
The nozzle lifts beads at corners or small islands High speed, fan starting too early Go back to the values in the first-layer table
Sticks, then hours later a corner lifts Shrinkage (warping), not a squish problem Bed, enclosure and brim: Warping and lifting corners
The material never grips that surface Wrong plate or no glue Beds and build surfaces, Bed prep for each material
Sticks too hard and tears chunks out of the PEI PETG on smooth PEI Textured plate or glue as a release agent, nozzle a little further away
Tall, narrow part that topples Small footprint; not a squish problem More contact area or a different orientation: Brims, rafts and mouse ears

How to test it

The quick check takes two minutes: print single-layer squares about 20 × 20 mm in the four corners and the center of the plate, or the first-layer test in your slicer's calibration menu if it has one. Compare all five with the three descriptions under "Reading a first layer": if they all fail the same way, adjust the Z offset; if they differ, check the mesh and the plate.

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?