kapy academy

Reading a failed print

17 min readUpdated Nov 2026

The part left on the plate is the only complete record of that print: because FDM builds layer by layer, every defect is recorded at the height and spot where it happened, in the order it happened. Read it before you reprint: a blind reprint buries the evidence. Answer three questions in this order: where the failure is (height and XY position), when it happened (which layer, and whether it is always the same one) and what it looks and feels like. With those answers, find its row in the symptom map. If two defects appear together, fix the lower one first.

Collect the evidence before you touch anything

Do not pull the part off or re-slice yet. Look at it in place first: whether it is still stuck down, where it came loose and whether there is a nest of plastic on the nozzle tell you more than the part will once it is off the plate.

Take one photo under raking light (a lamp or your phone torch held almost parallel to the wall) and one straight on. Under-extrusion, ringing (echoes after corners), VFA (fine vertical stripes) and Z-banding leave relief only a few hundredths of a millimeter deep. Head-on you cannot see it; with the light skimming the wall it jumps out. When you reprint with a change, the before photo will be your only reference.

The same wall of a gray PLA box. On the left, lit head-on, it looks smooth. On the right, under raking light, the layer lines, a few ripples after the corner and a thinner band all show up.
The same wall of a gray PLA box. On the left, lit head-on, it looks smooth. On the right, under raking light, the layer lines, a few ripples after the corner and a thinner band all show up.

With callipers, measure the height where the failure starts, from the face that sits on the plate, and turn it into a layer number. With the usual profiles for a 0.4 mm nozzle the first layer is 0.20 mm, so layer ≈ (height − 0.20) / layer height + 1. Quicker: drag the slider in the slicer preview to that Z and read off the layer. If you printed on a raft, add its height. Look at the preview at that layer:

  • If it already shows the problem, the cause is in the file: settings or geometry. For example, a missing wall, a gap in a thin section, a travel move across empty space, an island that starts in mid-air or a support that stops short.
  • If it is clean, the slicer did its job and the cause is in the machine, the material or the calibration. It is the check What a slicer does describes.

Check the spool and the filament path. Look for a wrap crossed over another, a flat spot chewed by the extruder gear, brittle filament snapping inside the tube, or crackling and steam at the nozzle. On a filament changer (AMS, MMU, CFS), check the history or the screen to confirm that the change at that layer actually happened. All of these produce a failure "from this height upwards" that no slicer setting fixes.

If your printer has a camera, go through the timelapse; check the error log too. A pause, a runout, a clog error or an alert pins down the exact moment. As of late 2026, some machines, such as Bambu's H2 series, use the camera or the extruder's force sensor to watch for three things: spaghetti, plastic building up on the nozzle and "printing in mid-air". External systems such as Obico or SimplyPrint do something similar from a webcam. All of them catch obvious failures and raise false alarms, and none of them diagnoses anything. How they work and how to set them up is covered in Sensors, cameras and failure detection.

Finally, touch it and break it. Notice whether the surface is rough or sharp, whether the wall gives, and above all how it breaks. A clean split along a layer line, with a smooth, shiny face, means weak bonding between layers. A fibrous break, with torn strands, means the part was overloaded.

Height is time: where and when

Every height on the part corresponds to a moment in the print. How the defect is spread along the height tells you what kind of cause to look for.

bednominal outlineOnly at the basefirst layer, bed, shrinkageAt one layeran event: crash, change,pauseFrom one height upsomething failed: clog,filamentPAt intervalsa period: lead screw, cycleOver the whole parta constant: flow,temperature, fan
Five patterns of the same defect along the height. Only at the base, at one layer, from one height upwards, at regular intervals or over the whole part: each points to a different kind of cause.
  1. Only at the base: the first layer, the plate, bed temperature or shrinkage pulling on the base. This is elephant's foot and warping territory.
  2. At a single height, then it recovers: a one-off event at that layer. A layer shift, a filament change, a pause, a bridge or an overhang that starts there, a brief clog that cleared itself.
  3. From one height upwards, getting worse: something stopped working and never came back. A clog or heat creep, a tangle on the spool, wet or chewed filament, a runout, a part that came loose, a curled overhang the nozzle hits on every layer.
  4. At regular intervals in Z: a mechanical or thermal period. Measure the spacing between bands: if it matches the lead of the screw (8 mm on the usual T8), it is the screw or its coupler; if not, suspect a bed temperature cycle.
  5. Over the full height, evenly: a constant. Flow, temperature, cooling, a speed beyond what the hotend can melt, or a design feature such as a thin wall.

The XY position counts as much as the height:

  • Always in one corner or on one side: the part-cooling fan (the side facing away from its duct), a draft in an open printer or one corner of the bed.
  • Right after a sharp corner or a hole, fading along the wall: ringing, a vibration.
  • In a straight line, layer after layer: the seam.
  • Only on small islands or thin towers: too little layer time to cool down, or too little contact with the plate.

Does it always fail at the same layer? If the part prints quickly, reprint the same file unchanged. If not, cut the model with the slicer's cut tool (Orca, Bambu Studio and PrusaSlicer all have one) and keep a band around that height. A band only tests faults in the file or the local geometry: it starts on the plate, is quick to print and stays short, so it never reproduces heat creep that builds over hours or the wobble of a tall part. If you suspect heat or time, print the whole file again.

  • Same layer, same spot: the failure is deterministic. It is in the file: geometry, settings or G-code.
  • A different height each time: it is mechanical, thermal or the material. Belts, a binding axis, heat creep that grows with time, a spool that snags.

Elapsed time matters too. A failure that turns up two or three hours into a PLA print in an enclosed printer is the classic heat creep symptom: the chamber warms until the cold side of the hotend is no longer cold and the filament softens too early. In an enclosed printer, open the door for PLA, PVA or TPU once the bed is above about 45 °C, and for PETG above about 70 °C (Enclosures and heated chambers). Diagnosis and cleaning are covered in Extrusion problems.

The symptom-to-cause map

Each row gives the most common cause on a modern, well-calibrated printer. The linked article explains how to rule out the others.

Two wall hooks printed on the bed, one upright and one lying, with the six most common defects marked: elephant's foot and warping at the upright hook's base, a layer shift and under-extrusion on its arm, ringing on the lying hook's wall and stringing between the two. Then a fresh print and the defects one at a time, with where they show and what causes them.
Six defects on the same two hooks, each where it usually shows. The ones at the base (elephant's foot, warping) come from the first layer and from shrinkage; one at a single layer is an event; one that starts at a height and carries on upward is something that stopped working; one that follows a corner is a vibration; stringing is oozing between travels. The defects are exaggerated and the layers drawn thicker so they show.
Symptom, likely cause and where to fix it
What you see Most likely cause Go to
Base wider than the rest, holes narrow near the plate Elephant's foot: first layer squashed too hard The first layer and bed adhesion, The face on the bed
The part did not stick or came off early, with well-extruded lines Dirty plate, Z offset, bed temperature The first layer and bed adhesion
A corner lifting after a few good first layers Shrinkage pulling on the base Warping and lifting corners
PETG tore chunks out of the plate Too much adhesion on smooth PEI Bed prep for each material
The part split along a layer, cracks between layers Weak bonding: cold, too much fan, wet filament, ABS/ASA without an enclosure Layers splitting apart
Hairs and cobwebs between features Stringing, oozing, wet filament Stringing and blobs
Zits and blobs at the same spot on every layer Seam, retraction Stringing and blobs, Where the seam goes
Gaps between lines or between wall and infill, thin walls, a clicking extruder, a part that thins as it rises Under-extrusion, partial clog, heat creep, flow limit Extrusion problems
Rough surface with excess material, ridges, nozzle dragging Over-extrusion Extrusion problems
Holes or pillowing on top faces Too few top layers, under-extrusion Top surfaces
Echoes after corners, fine vertical stripes, regular horizontal bands Ringing, VFA, Z-banding Wall marks: ringing, VFA and Z-banding
Dimensions that do not add up, small holes, fits that fail Shrinkage, flow, polygonisation Parts that print the wrong size
Overhang drooping or curling upwards, sagging bridge Cooling, angle, speed Overhang and bridge failures
Layers stepped sideways Layer shift: crash into a curled overhang, belt, acceleration Layer shifts and spaghetti
A nest of plastic where the part should be Spaghetti: loose part or extruding onto nothing Layer shifts and spaghetti
Contaminated colors at the transition, a change that did not happen, filament stuck in the changer Changer or purge failure Multi-material failures

Wet filament impersonates half the table: crackling or hissing at the nozzle, steam, strings, a rough or fuzzy surface, weak layers and bubbles in the bead. If you see any of them with PETG, PA, PC, TPU or PVA, dry the spool and print again before you hunt for another cause. At least eight hours: PETG at 60–65 °C, PA at 80–85 °C, PC at 80 °C, PVA at 75–85 °C and TPU at 70–75 °C, TPU for up to 18 h. The full procedure is in Drying and storing filament.

A symptom that is not in the table is usually two rows at once.

When two failures mix: where to start

Failures set off other failures, and the most visible one is usually the last in the chain. A poorly cooled overhang curls upwards. On the next layers the nozzle hits the curl. The impact makes a motor skip steps (a layer shift) or knocks the part loose. The rest of the print is spaghetti. What you see is spaghetti; the cause is the overhang. Read the part from the bottom up and fix the lowest defect.

diagram
The failure you see is the last link. Clearing the spaghetti does nothing: the overhang that started the chain needs better cooling.

There is one exception. Warping and lifting sit at the base, but they happen late, often hours in, as the part shrinks or the chamber cools. A corner that lifts mid-print can cause a crash higher up. If the base has lifted, check the timelapse for when it lifted.

When the part does not make the order clear, work through the causes in this sequence, from the most basic to the most specific:

  1. Material: the right profile for that filament, the filament dry and the spool turning freely.
  2. Plate and first layer.
  3. Extrusion: flow, temperature, no partial clog, and a speed the hotend's volumetric flow can sustain.
  4. Cooling.
  5. Motion: belts, ringing, shifts.
  6. Slicer settings for that particular feature.
  7. Design.

The order matters because a cause near the top mimics the ones further down. A partial clog looks like poor cooling, weak layers and a dimensional error all at once. Nothing at the bottom of the list fixes a cause at the top. Speed is the classic example: the ceiling is the hotend's flow, speed = flow / (line width × layer height), and a 21 mm³/s hotend tops out at 233 mm/s with a 0.45 × 0.20 mm bead (Volumetric flow sets the speed). Beyond that, the profile asks for more plastic than the hotend can melt, and that is under-extrusion even when everything else is right.

To break a tie, use where and when:

  • A part that comes out the wrong size. If the error grows in proportion to size and is everywhere, it is shrinkage. If it is a constant offset, say +0.2 mm on every outside dimension whatever the size, it is flow or line width. If it only affects the first few tenths of a millimeter of the base, elephant's foot. If it only affects round holes, polygonisation and squash: a small hole comes out 0.1 to 0.3 mm too small in diameter even on a calibrated machine.
  • A rough surface. Rough everywhere means over-extrusion. Fuzz, strings and bubbles mean wet filament. Only along the travel moves, strings flattened by the nozzle.
  • Separated layers. A smooth, shiny face means weak bonding, often at a specific height on a tall part or near the top of a part with very fast layers. A fibrous, torn break is overload. In a sound part, Z strength is about half of XY (30 % fiber-filled); with long layer times, heavy fan, wet filament, or ABS, ASA, PC or PA in an open printer, it can fall to 20–40 % (Layer adhesion and anisotropy). The physics and the fixes are in Layers splitting apart.

Change one thing at a time. Reprint the smallest part that shows the defect and write down what you changed. Three changes and one success teach you nothing you can repeat on the next part. The exception is the baseline: a clean plate, dry filament and the manufacturer's profile are not variables. Get all three right before you experiment.

Some failures you stop rather than study: a nest growing on the nozzle, plastic wrapping the heater block, the part being dragged along by the nozzle or a scraping noise from the axes. Stop the print. If there is a blob on the block, heat the hotend to printing temperature to soften it and pick it off with tweezers, without pulling on the wires. If the silicone sock or the thermistor or heater wires are damaged, replace them before printing again. If you smell burning or see smoke, do not clean anything: cut the power. Why an unwatched failure is a safety problem is covered in Fire risk and unattended printing.

What belongs to the design and what to the machine

The test is one question: would this fail on any well-calibrated printer? If yes, the problem is in the geometry. For example: an unsupported ceiling, an overhang beyond the machine's angle, a wall thinner than two lines, a tall narrow part on a small footprint, a fillet on the edge that sits on the plate, a detail smaller than the nozzle, or a load that tends to pull the layers apart. If it failed on one printer or with one spool and not another, it belongs to the machine or the material.

Design signs: the failure lines up with a feature of the geometry (it starts where an overhang or an island starts, in a thin section, at a sharp corner of the bed face), it repeats at the same layer every time and the preview shows it. Machine signs: it changes height between prints, covers the whole part evenly, sits on one side of the bed or appeared after a nozzle, spool or plate change.

It is nearly always a bit of both. A 50° overhang prints fine on a modern machine with an auxiliary fan or cooling from both sides, and droops on a legacy bedslinger with a single fan on one side. A fix in the design travels with the part to any printer; a fix in the machine only works on yours. Choose the design fix if other people will print the part or you will print it on other machines. Choose the machine fix if the failure shows up in everything you print.

When it fails

When the reading does not lead to the fix
Symptom Cause Fix
You change a setting and the failure stays the same You fixed the most visible defect, not the lowest one in the chain Read the part from the bottom up and fix the first defect that appeared
The cut-out band prints fine and the whole part fails The failure depends on time or heat: heat creep, a tall part wobbling Print the whole file again; on an enclosed printer, open the door as the material requires
After several changes the part prints fine, but the next one fails again You changed several things at once and do not know which one fixed it Go back to the starting profile and change one thing at a time
The failure appears at a different height on every attempt A mechanical, thermal or material cause, not the file Check belts, axes, spool and filament before the slicer (What to calibrate, and in what order)
The design checks flagged nothing and the part breaks between layers A load that pulls the layers apart, which those checks do not cover Reorient the part so the load runs along the beads (Layer adhesion and anisotropy)

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?