Every bead needs something underneath it. Wherever a face sticks out past the layer below or spans a gap, the plastic has to hold its shape in mid-air until it sets; when it cannot, it leaves a mark, and each mark points to a different cause. These are geometry failures, and they are nearly always fixed in the geometry. Check the angle and the span first, then air and heat, then the slicer's settings (Overhang and bridge settings) and, last, support and the scar it leaves (Support settings).

Identify the failure

BedDroopNozzleCurlSagAnchorBroken strandTeardropSunken roof
Five marks in cross-section. Anything that hangs down is missing cooling or support; anything that rises above the layer is curl; a bridge that bows along its length is not the same as one that broke.

Look at the part from below and from the side under raking light: your phone torch held almost parallel to the face, as in Reading a failed print. Three questions sort out nearly any case. Does the defect fall (droop, sag) or rise (curl)? Is it on a sloping face (overhang), across a gap anchored at both ends (bridge), or on a face that sat on support? Is it the same all the way round, or worse on one side?

Before you blame the printer, open the slicer preview colored by line type. Overhang walls and bridges have their own colors, and three file errors show up there: a bridge laid along the length of a slot, a "bridge" the slicer drew as an overhang because one end has no anchor, and a missing support. If the preview already shows the problem, the cause is in the file.

The drooping underside

The underside of a sloping face comes out rough and wavy, and gets worse as it approaches horizontal. Where the slope is flattest, loops and curtains of plastic hang down. The upper part of the slope, closer to vertical, comes out clean.

Each bead of the outer wall sticks out past the one below, and the part left in the air has nothing to hold it up or to cool it: it stays soft for longer and gives way before it sets. With 0.20 mm layers and 0.45 mm beads, 44 % of the bead hangs in the air at 45°, 77 % at 60°, and the whole bead from about 66° onwards. Design overhangs at 45° measured from the vertical; any steeper angle your machine handles is for your own parts (Orientation and overhangs).

Note the angle where it starts. If it begins past 45° on a legacy bedslinger, or past 50–60° on a modern machine with PLA, the machine is fine: the face asks for more than the machine can print unaided. If a 40–45° face droops, something else is wrong: cooling, temperature or settings.

The fixes, in order:

  1. Reorient so the face stands vertical or faces up. It costs nothing (Orientation and overhangs).
  2. Change the geometry. A 45° chamfer instead of a flat shelf; on the bottom edge, a chamfer rather than a fillet, because a fillet starts out almost horizontal (Designing out supports).
  3. More air on the overhang. With PLA, fan at 100 % on overhangs, and check the angle at which it kicks in. With PETG, raise the overhang and bridge fan to 50–90 %; with ABS and ASA, up to 80 %, on overhangs only.
  4. Nozzle 5 °C cooler, within the material's range (PLA 190–230 °C, PETG 230–270 °C). Hotter plastic is runnier and takes longer to set.
  5. Slower overhang speed bands or thinner layers for that section: the same angle with a smaller step per layer. Points 3 to 5 are set in Overhang and bridge settings.
  6. Only then, support.

Also rule out what makes it worse. Wet filament leaves bubbles and a rough, fuzzy skin on the overhang: dry it before you touch anything else (Drying and storing filament). Over-extrusion puts more plastic into each bead than can stay put (Extrusion problems). With outer-to-inner wall order, the outer bead has no inner wall to lean on and droops sooner: go back to inner-to-outer, or use inner-outer-inner if your slicer offers it. And PETG and ABS manage 5–10° less than PLA: an angle proven in PLA is not proven in PETG.

The curling overhang

The edge of an overhang, the bow of the Benchy or the rim of an inverted cone lifts above the plane of the layer and forms a lip that stands a few tenths of a millimeter proud of the next layer. You can often hear the nozzle strike or scrape it on every layer, and the crest of the lip goes shiny from the rubbing.

A curled overhang: the edge of the last few layers lifts above the layer and the nozzle scrapes it on every pass (generated illustration)
A curled overhang: the edge of the last few layers lifts above the layer and the nozzle scrapes it on every pass (generated illustration)

This is not droop. The hanging bead cools from the top first. That face shrinks and pulls the free edge upwards, like a bimetallic strip. Each new layer goes down on an edge that has already lifted and makes the lip bigger. It is worse in ABS and ASA, which shrink more; in PETG, which prints with far less fan and comes out hotter and stickier; and on fast outer walls, where the bead is laid down stretched.

Curl matters more than droop because it is the start of a chain. The nozzle hits the curl, a motor skips steps or the part breaks free, and the rest of the print is spaghetti (Layer shifts and spaghetti).

With PLA, the fix is more air on the overhang, so the bead sets before it can move. OrcaSlicer has "Slow down for curled perimeters", which slows down where earlier layers have lifted, and "Reverse on even", which reverses the direction of overhanging walls on alternate layers so each pass cancels the pull of the one before. PrusaSlicer's dynamic speeds also slow down over curled edges, and its "Avoid crossing curled overhangs (Experimental)" routes travel moves away from the lip. Those are the names as of late 2026; the details are in Overhang and bridge settings. With ABS and ASA: an enclosed printer, a low part-cooling fan and up to 80 % on overhangs only, never with the fan off. Z hop on travel moves reduces the strikes but does not remove the lip: it is a workaround.

If the curl starts at the bed and lifts the base, it is warping (Warping and lifting corners). If it starts on an overhang, partway up the part, it is curl.

One side comes out worse than the other

AirCleanDroopingSingle blowerRotate the part: the defect follows the duct, not the partEvenRing or dual duct
The same round overhang seen from above. With a single blower, the side away from the duct droops; with air from both sides, the edge comes out the same all the way round.

If a round overhang comes out well on one side and badly on the other, the cause is the air, not a setting. A single blower on one side of the toolhead, common on many legacy bedslingers, cools the opposite side much less well. That machine's 100 % is much less air than 100 % on one with ducts on both sides (Speed and cooling). A cracked duct, one clogged with plastic or one knocked out of place leaves the same mark on a machine that used to print that part well.

Check that the fan spins and that the duct is clean and properly seated. Rotate the part so the critical overhang faces the duct. On a legacy machine, a better duct is the upgrade you will actually notice. Machines such as Bambu Lab's enclosed models have far more air: a large part-cooling blower and an auxiliary side fan. That auxiliary fan blows from one side of the chamber, and that draft is exactly what hurts ABS and ASA: leave it off with them (Layers splitting apart).

The very-fast-layer trap. A small part, the tip of a cone or a thin finger with an overhang prints each layer in a second or two. The nozzle comes back over plastic that is still soft, and the overhang melts and bends even at a modest angle. The problem is heat build-up: minimum layer time, more copies on the plate or a sacrificial tower (Speed and cooling).

Bridges that sag or break

From a distance they look alike; tell them apart before you change anything.

Sag. The strands are continuous and anchored at both ends, but they bow downwards in the middle. The first bridge layer is the worst; the layers above partly flatten it. How far your machine bridges without support, and with which settings, is in Overhang and bridge settings. If the span is within that, the causes are too little air, plastic that is too hot, or too much flow, which leaves the strand slack. Shorten the span in the model with a rib in the middle, or a 45° pitched roof instead of a flat one (Designing out supports); run the fan at 100 % on bridges with PLA; lower the bridge flow ratio from 1.0 toward 0.95; use "Thick bridges" if that face will not be seen.

Broken or missing strands. Strands snapped in the middle, torn off an anchor, or with gaps between them. Causes: the strand was jerked (bridge speed or acceleration too high for the anchor), flow so low the strand breaks, or a weak anchor because the bridge starts on sparse infill or on a single thin wall. Lower bridge acceleration and speed, bring the flow back toward 1.0 and thicken the wall where it anchors. Slowing down has a limit: a strand laid too slowly cools before it is pulled taut, and it hangs. Print the bridge slower than the walls, but neither at 10–15 mm/s nor at full speed.

Wrong direction. The strands run along the long side of a slot or a window, and each one is far longer than the width of the gap. Or one end of the "bridge" has nowhere to anchor and the slicer prints it as a curtain of overhang. Both show up in the preview. Set the bridge angle by hand, or give the area a second anchor in the model. A ceiling held at one end only is not a bridge: it needs support, a redesign or "Extra perimeters on overhangs", which closes it by growing out from the supported edge, slowly, and leaves rings on the underside.

If the wall right after the bridge comes out thin or with a short gap, the problem is pressure: check pressure advance on bridges in Overhang and bridge settings.

Holes, counterbores and internal bridges

An oval horizontal hole. Its top flattens or sinks and the hole comes out narrower at the top. The roof of a round hole is a short bridge with very steep overhangs either side. A horizontal hole up to 6 mm prints clean; between 6 and 10 mm the roof sags 0.1–0.3 mm, acceptable except in a pivot or a precision hole; above 10 mm, draw it as a teardrop or with a flat roof (Designing out supports). The teardrop has 45° sides and the point at the top, truncated flat if the hole has to be accurate. The other reasons a hole comes out narrow are in Why holes print small.

A ring of loops under a counterbore. A counterbore for a screw head or a nut trap above a through hole leaves a ring-shaped step with nothing underneath, and its first layer hangs in loops. Add a sacrificial layer, either modeled (Captive nuts and clearance holes) or with OrcaSlicer's "Bridge counterbore holes" → "Sacrificial layer", then drill through it.

Bumps and pinholes on a top face. The first solid layer over infill is an internal bridge that sagged. It is covered in Top surfaces.

The surface the supports ruined

Orientation decides which face pays for the support. When something still goes wrong, the face tells you what failed.

The underside still droops or is ridged even though it had support. The top Z distance is too large or the interface too sparse, and the first layer over the support prints almost like a bridge. Bring the top Z distance down to one layer height (0.2 mm with 0.2 mm layers), use 3 interface layers and reduce the interface line spacing.

The support fused to the part and tears the face off when you remove it. Top Z distance too small, interface too dense, PLA too hot, or PETG printed with PLA's distance. Raise the top Z distance by 0.05 mm (with PETG, more than with PLA: start at about 0.25 mm) and widen the interface line spacing. On a machine with a filament switcher, an interface in a material that will not bond (PETG under PLA, or the other way round) avoids the problem (Support settings).

The support fell over or came loose mid-print. Then the overhang above it printed in mid-air, and you see it as droop or as a layer of spaghetti at a single height. Causes: thin tree branches on a tall support, a support base that peeled off the bed, or the nozzle striking a curled overhang. Thicken the branches or add a brim under the support, and check adhesion under the support's footprint (the section on the support base in Support settings).

Side faces marked where the support touched. The XY distance is too small: raise it (Support settings).

The scar on a face that should have come out smooth. A setting rarely fixes it: orientation does. Orient the visible face up or vertical, leave the scars on a hidden underside and block support where it is not needed. To remove and clean up what is left: Support removal and cleanup.

Would it fail on any machine?

The test from Reading a failed print: would it fail on any calibrated machine? An overhang beyond 60–70° with no support or redesign, a flat bridge longer than 50 mm, a ceiling anchored on one side only, or a horizontal hole over 10 mm without a teardrop: yes. That gets fixed in the design, and tuning the slicer only wastes filament.

When it fails

Symptom, cause and fix
Symptom Cause Fix
Rough, drooping underside on a slope Angle beyond what the machine prints, too little air or plastic too hot Reorient or chamfer; overhang fan; −5 °C; slower overhang speed bands or thinner layers
Edge lifting, nozzle strikes it The top of the hanging bead shrinks More air on overhangs (PLA); "Slow down for curled perimeters"; "Reverse on even"; enclosure and moderate fan with ABS and ASA
One side of a round overhang worse than the other The air does not reach that side Check fan and duct; rotate the part
Small part melts and bends at a low angle Heat build-up Minimum layer time; more copies on the plate
Bridge sagging in the middle Long span, too little air or too much flow Shorten the span; fan at 100 % (PLA); bridge flow from 1.0 toward 0.95; "Thick bridges" if hidden
Strands broken or torn off the anchor Speed or acceleration too high, flow too low, weak anchor Lower bridge acceleration and speed; flow back toward 1.0; thicker anchor wall
Strands along the long side, or a curtain on a "bridge" with one anchor Direction or anchoring Bridge angle by hand; second anchor; support
Horizontal hole narrower at the top, with a flat roof The hole's roof is a bridge Teardrop above 10 mm, or from 6 mm if the hole must be accurate
Ring of loops under a counterbore The step has no anchor Sacrificial layer
Bumps on a top face Sagged internal bridge Top surfaces
Droop on a supported face Top Z distance too large One layer height; 3 interface layers
Support fused to the face Distance too small, or PETG printed with PLA's distance Raise it 0.05 mm; with PETG, more than with PLA
Overhang printed in mid-air at a single height The support fell over Thicker branches; brim under the support

How to test it

Do not guess your machine's envelope, meaning the angles and spans it prints cleanly: measure it. Print once per material, with your usual profile, an overhang test stepping every 5° from 30° to 70° and a bridge test from 10 to 50 mm; the procedure is in Overhang and bridge settings. When you tune something, change one thing per test print.

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?