kapy academy

Coatings and epoxy

14 min readUpdated Nov 2026

Coat a part when you want gloss without sanding to a mirror, a part that holds water, or a surface that stands up to sunlight, rubbing and greasy hands: you add a film on top. Sanding takes material away and vapor moves it around; a coating adds it, so every dimension grows outwards and mating faces are masked first. No coating makes a part food-safe on its own. Start from a clean part (Support removal and cleanup) and, almost always, one you have already sanded once (Sanding and smoothing).

Choosing the coating

To level and gloss, use one or two thin coats of low-viscosity 3D-printing epoxy, brushed on, each under 0.4 mm. To protect without changing the look, use a clear aerosol varnish, which leaves a few hundredths of a millimeter per coat. To seal small parts, use thin cyanoacrylate.

Each class behaves differently for a physical reason. A leveling coating flows: it has low viscosity and gels slowly, so surface tension pulls the liquid flat across the valleys before it hardens. A varnish is mostly solvent or water that evaporates and leaves a thin film that copies the surface underneath. That is why leveling epoxy erases the layers and varnish does not.

Coating classes for FDM parts (indicative manufacturer values)
Class What it does Film per coat Cure Watch out for
3D-printing epoxy (two-part, self-leveling, brushed; e.g. XTC-3D) Fills valleys and levels the layers with a hard gloss Up to ~0.4 mm, uneven Pot life ~10 min; tack-free ~2 h; full cure ~3.5–4 h at 23 °C Exact ratio, heat of the mix in the cup, sags on the bottom edge
Table-top epoxy (such as ArtResin) Pours of about 3 mm that level themselves Millimeters Hard in 24 h; full cure at 72 h Drips and buries detail: flat display faces or filling a recess only
Clear varnish or lacquer (acrylic or polyurethane, water- or solvent-based) Protects against UV, rubbing and dirt; matt, satin or gloss ~10–30 µm dry per aerosol coat; 25–75 µm brushed Minutes to touch, hours between coats The layers still show; outdoors, use a UV-resistant one
Thin cyanoacrylate Wicks between the layers of small parts and hardens the skin Almost none Seconds White frosting (blooming) around it, brittle, heats up suddenly on cotton
Leftover photopolymer resin (from a resin printer), brushed Hard, glossy film in minutes Thin Under UV light Brittle; uncured, it sensitizes skin; not food-safe; cures only where the light reaches
diagram
Choose the coating by the job it has to do, not by the finish it promises.

Epoxy gives off heat as it cures, and in a thick mass that heat cannot escape. Table-top resins are formulated to stay cool in layers of about 3 mm. The real risk is in deep-pour casting resins, in pours thicker than about 6 mm and in the mix left sitting in the cup: there the temperature can soften PLA. The varnish here is the same clear coat that finishes a paint job (Painting and priming). Cyanoacrylate heats up suddenly on contact with cotton: no rags and no cotton gloves. Handle photopolymer resin as described in Handling resin safely; epoxy as an adhesive is in Gluing and welding printed parts.

How much thickness it adds and where it builds up

A coat does not leave a uniform thickness. The resin spreads according to the shape, and that decides which dimensions change.

copies the surfacevarnishfills the valleysthin on the crestssaggravityepoxythe hole closesthin on the edgepools in the corneredges and holes
Varnish copies the layers at constant thickness. Epoxy fills the valleys and stays thin on the crests, on sharp edges and over small holes, and builds up in inside corners and on the bottom edge.

Across the layer profile, epoxy leaves several tenths of a millimeter in the valleys and only a thin film on the crests. On a convex edge, surface tension pulls the liquid back, so edges stay thin and are the first thing to wear through. In an inside corner the liquid pools and rounds it off. Holes, slots and engraved text of half a millimeter or less usually fill in. On vertical faces the resin sags and leaves a thick bead along the bottom edge.

The same part uncoated and with one coat of epoxy: the layers vanish under the gloss, and a sag bead remains on the bottom edge (generated illustration)
The same part uncoated and with one coat of epoxy: the layers vanish under the gloss, and a sag bead remains on the bottom edge (generated illustration)

The design consequences are the same as for paint, with bigger numbers. Engraved or embossed text softens, a small hole closes and a sliding fit binds. The film grows on both faces of a gap: 0.3 mm of resin on each wall of a slot eats 0.6 mm of its width, more than the 0.4 mm total clearance of a 0.20 mm-per-side sliding fit (Real printed clearances). Coat the tongue that goes into it as well and you lose 1.2 mm.

The fix is to mask fits, holes and threads with tape or plug them with a greased pin or a printed stopper, or to add the film to the model. In KapyCAD, dimension fields accept formulas, so you can create your own parameter for the coating thickness next to the fit constant: a hole of 5 + 2 * FIT_SLIDE + 2 * COATING (Tolerances in the Model).

One coat adds a few grams to a palm-sized part and some surface hardness. It adds no structural strength, does not fix poor layer bonding and does not raise heat resistance: coated PLA still softens near its 57 °C heat deflection temperature (HDT at 0.45 MPa). That is the job of Annealing and strengthening.

Sealing: watertight parts

An FDM part leaks through the tiny gaps between beads and between walls, above all at the seam and where the walls meet the top or bottom skins. Water gets through by capillary action even when the part looks solid.

Fix it in the print first, then coat. Add more walls and more top and bottom layers, put the seam in a corner and avoid under-extrusion (Walls, perimeters and infill, Extrusion problems). A coating plugs isolated pores; it does not rescue a porous print.

Coat the face that touches the water: the inside of the vase, container or tank. Pour in a little low-viscosity epoxy, swirl it or brush it into the corners, then coat the outside if it has to look good. Two thin coats beat one thick one, because a thick coat traps bubbles that later become pores.

Test it before you use it. Fill the part with water and leave it overnight on kitchen paper. For a part that must hold air or pressure, such as an electronics enclosure or a pneumatic part, do a bubble test with soapy water.

Rigid coatings crack on parts that flex. Epoxy on TPU or on a thin wall that flexes in service crazes, and the part starts leaking again. On flexible parts, trust the print: TPU printed slowly with good flow seals well. Hot water is fine for the epoxy, but the PLA beneath it starts to soften at 55–57 °C.

Food contact: how far a coating goes

A part straight off the printer is not food-safe. The gaps between beads harbor bacteria, brass nozzles can contain lead and the colorants are not certified. A coating closes those gaps and becomes the surface that touches the food. That is why it is the usual route for a mug or a bowl, but it only works if four conditions hold:

  1. The product declares food-contact compliance in its cured state, for your market. In the US, manufacturers declare compliance with 21 CFR 175.300; the FDA does not approve or certify finished kits. In the EU the framework is Regulation (EC) 1935/2004, with a declaration of compliance from the manufacturer. On top of that, Regulation (EU) 2024/3190 bans bisphenol A in food-contact varnishes and coatings, and its general transition period ended in July 2026. Almost all table-top and printing epoxies are made from bisphenol A, so a claim of compliance with 21 CFR 175.300 says nothing about compliance in the EU. In the EU, assume a consumer epoxy is not food-safe unless the manufacturer supplies an EU declaration of compliance that cites that regulation. Some manufacturers also limit compliance to brief or occasional contact: read the label.
  2. Full cure, as the datasheet states. ArtResin, for example, asks for 72 h; others ask for seven days. The product datasheet rules. Undercured resin migrates. A fast 3D-printing epoxy is not food-safe unless the manufacturer says so.
  3. A continuous film. Every surface that touches food coated, with no pores and no bare edges. Check it under raking light.
  4. Use within the limits. Cutlery and scourers scratch the film and expose the layers beneath. Dishwashers and hot drinks soften the PLA underneath. Wash by hand, cold or lukewarm only, or print in a material that takes more heat. Inspect the part regularly and replace it as soon as the film is scratched.

Certified material, the stainless steel nozzle and easy-to-clean design are in Printing for food contact.

Applying epoxy, step by step

Prepare the part. Remove every trace of support, because a gloss coat shows up every one. For a mirror finish, sand the worst layers first: one coat levels the valleys of a 0.2 mm layer, not large steps. Remove the dust, degrease with isopropyl alcohol and let it dry. Mask fits and holes. Decide where the part will rest while it cures: on points, on a printed stand or hung from a wire through a hidden hole, with the face that matters facing up.

Prepare the workspace. Work between 20 and 25 °C, with ventilation, nitrile gloves and safety glasses. Epoxy sensitizes the skin, and sensitization lasts for life. Wear a dust mask when you sand cured epoxy.

Measure and mix. Stick to the exact ratio, by weight if you can. For XTC-3D, for example, it is 100:42 by weight or 2:1 by volume. With the wrong ratio the mix never fully cures, and extra hardener does not speed it up. Mix for at least a minute, scraping the sides and bottom.

Control the heat of the mix. Epoxy heats itself, and faster in a deep cup. A large mass can melt a plastic cup or burn skin. Mix small batches, what you can spread in about ten minutes, and tip it into a flat tray to extend the working time. For the same reason, no thick puddles on PLA.

Apply thin coats. Use a foam brush and keep working the surface until the mix starts to gel: brushing off the excess is what prevents sags. On complex parts, work one face at a time. Pop surface bubbles with a brief pass of a heat gun or torch, held well back and moving, because PLA softens near 57 °C.

Second coat. Apply it when the first is tacky but firm (about 90 min for XTC-3D in a thin film). If the first coat has fully cured, scuff it lightly first so the second one bonds. On PLA, do not speed up the cure with heat. The manufacturer offers a 60 °C cure and only warns that the part may melt above about 93 °C, but 60 °C is already above the HDT of PLA (57 °C at 0.45 MPa). ABS (87 °C) and ASA (100 °C) tolerate it; PETG (69–71 °C) is borderline: cure it at 60 °C only if the part is well supported and has no thin walls.

Final finish. For a matt finish, sand the cured epoxy lightly. For color, sand until the gloss is gone and paint (Painting and priming). For outdoors, add a UV-resistant clear varnish on top, because almost every epoxy yellows in sunlight.

When it fails

Symptom, cause and fix
Symptom Cause Fix
Still tacky the next day Wrong ratio, too little mixing or too cold Scrape off the soft resin, clean with isopropyl alcohol and recoat with a properly measured mix. Time will not cure it
Sags and a thick bead on the bottom edge Coat too thick or not worked Sand the bead flush once cured. Next time, go thinner and keep brushing until it gels, turning the part if you can
Bubbles and pores Air from the infill and the gaps between beads expanding as the part warms, or air stirred in while mixing Apply a thin sealing coat first, let it gel, then apply the gloss coat. Mix slowly and pass the heat gun over the surface
Craters or fish-eyes Contamination: silicone, grease, release agent, fingerprints Sand, degrease with isopropyl alcohol and recoat. Handle with gloves
Waxy or cloudy film (amine blush) Humidity or cold during the cure Wash with lukewarm water and a sponge before sanding or recoating
Part warped or sunken under the resin Heat from a thick pour or an oven cure on PLA Thin coats, small batches and no oven with PLA
Peels off Poor adhesion on smooth or low-surface-energy plastics: mediocre on PETG, almost none on PP and PE Sand until the gloss is gone and degrease. On PP, do not count on any coating (Polypropylene)
Yellows in sunlight Epoxy's sensitivity to UV. Those with UV stabilizers take longer, but none is immune UV-resistant clear varnish on top (Heat, cold, sunlight and chemicals)
Cracks on a part that flexes Rigid film on a flexible part Leave flexible parts uncoated or use a flexible coating

See also

Design it in KapyCAD

Many of these problems are cheaper to fix in the model than in the slicer: wall thickness, overhangs, the face the part stands on.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?