You print a PLA bracket with two Ø6 holes that have to land on two M6 tapped holes in an aluminum plate, 150 mm apart. Each hole measures fine, but the pattern comes up half a millimeter short and the second bolt will not go in. Every thermoplastic shrinks as it cools from the nozzle to room temperature, and every length shrinks by the same proportion: from 0.2–0.5 % for PLA to 1.5–2.5 % for PP. It is a scale error: a 5 mm hole barely changes, but a 150 mm pattern moves by several tenths.

Why it shrinks

A bead leaves the nozzle at 200–300 °C, and every plastic takes up less volume as it cools. What matters is how much of that shrinkage reaches the dimensions.

amorphous, still soft: flows and relaxesvolumetemperaturecoolingroomTgTc (crystallization)frozen: the shrinkage you seecrystalsamorphoussemi-crystalline
Above Tg (amorphous) or crystallization (semi-crystalline) the plastic still flows and absorbs the shrinkage. Whatever shrinks after that point is what changes the dimensions.

In an amorphous plastic, above the glass transition (Tg) the material is still soft enough to flow and relax: the bead absorbs almost all the shrinkage in that range as it settles. Below Tg the shape is frozen. Every degree it still has to lose becomes a shortening, and the bed and the lower layers pull against it. That is the shrinkage you see in your measurements, and the shrinkage that lifts corners.

Amorphous plastics

The higher the Tg, the longer the frozen stretch down to room temperature and the greater the shrinkage. PLA freezes at around 60 °C, ABS at around 105 °C and PC at around 145 °C. That is why ABS and PC shrink more than PLA even though they expand by a similar amount per degree: their temperature drop below Tg is two or three times larger. An unfilled plastic expands by about 70–100 µm per meter per degree. Multiply that by PLA's 35–40 °C drop and you get roughly 0.3 %; by ABS's 80 °C, 0.6–0.8 %. It matches the table in the next section. For PC the sum would give more, but its lower expansion per degree and the bed's restraint leave the real figure at 0.5–0.8 %, like ABS.

Semi-crystalline plastics

In semi-crystalline plastics (polyamides, PP, PEEK, PPS) the shape is fixed when the plastic crystallizes, well above its Tg: PP's Tg is below zero and a dry polyamide's is around 50 °C. On crystallizing, some of the chains fold into crystals, which take up much less space than the melt. That whole drop, plus all the cooling after it, ends up in the dimensions. That is where polyamide's 1–2 % and PP's 1.5–2.5 % come from. Their shrinkage also depends on how fast they cool: more crystallinity, more shrinkage. A hotter bed or an enclosed chamber changes the figure. On paper PLA is semi-crystalline too, but in printing it cools so fast that it comes out almost amorphous.

Fiber-filled composites

Short fibers barely shrink and hold the matrix back along the bead: 0.2–0.5 % in that direction, more across it and in Z.

If shrinkage is not uniform across the part, the layers pull on each other and the corners lift. Warping and lifting corners explains the mechanism and how to prevent it.

All of this applies to filament. A resin part shrinks as it cures and post-cures, not as it cools, and these figures do not apply to it: Types of resin covers it.

How much each family shrinks

Indicative linear shrinkage by family
Material Linear shrinkage Over 100 mm
PLA 0.2–0.5 % 0.2–0.5 mm
PLA-HT 0.3 % (annealing adds 1–5 % in XY) 0.3 mm
PETG, PCTG 0.3–0.5 % 0.3–0.5 mm
PVB 0.3–0.5 % 0.3–0.5 mm
ASA 0.4–0.7 % 0.4–0.7 mm
ABS, PC 0.5–0.8 % 0.5–0.8 mm
PC-ABS, HIPS, PEI 0.5–0.7 % 0.5–0.7 mm
TPU 0.5–1 % 0.5–1 mm
Unfilled PA6, PA12, CoPA 1–2 % 1–2 mm
PEEK 1–1.5 % 1–1.5 mm
PP 1.5–2.5 % 1.5–2.5 mm
PA-CF/GF, PAHT-CF 0.2–0.5 % along the bead (more across it) 0.2–0.5 mm
PET-CF, PPA-CF, PPS-CF 0.2–0.4 % along the bead (more across it) 0.2–0.4 mm

The table is an order of magnitude for printed parts, not a datasheet value. It varies with the brand, the color and pigment, the size of the part and the print profile. Filament datasheets almost never give shrinkage, and when they do it is usually the injection-molding figure, which is not yours (Reading a material datasheet).

Against a molding figure you will usually measure less: the bed and the lower layers hold the part back as it cools, so it shrinks less than the same part cooling unrestrained. Within the table, the top of each range belongs to large, solid or poorly anchored parts. A small, thin part in the same filament sits lower.

In practice, brands within a family differ by a fraction of the range; between families the difference is several times larger. If you change family, measure again. Choosing a filament works through a Ø20 hole when you switch from PLA to nylon.

A scale error, not an offset

Shrinkage multiplies every length by the same factor, (1 − s). Two consequences follow. A hole and a pin of the same size lose the same amount, and it is tiny. What loses a lot is a long dimension: the distance between holes, the overall length, the spacing between two faces that bear on another part.

hole spacingloses s × Lmetaldoes not fitholeloses s × d (tiny)nominalshrunkshrinkage exaggerated
Shrinkage scales the whole part. Each hole loses hundredths, the distance between them loses tenths, and against a metal bar only the distance fails.

A Ø5 hole in PLA at 0.4 % loses 0.02 mm, within the reading noise of a hobby calliper. Two holes 150 mm apart move 0.3–0.75 mm closer in PLA and 0.75–1.2 mm in ABS. A sliding fit on a modern machine takes 0.15–0.20 mm of clearance per side. The hole fits; the pattern does not.

A small vertical hole prints 0.1–0.3 mm tight on the diameter because of facets, the bead bulging into the curve and shrinkage (Why holes print small), and in a small hole shrinkage is the smallest of the three causes. Do not fix it with a scale: at 0.4 %, a Ø5 opens up by 0.02 mm.

Between printed parts the error largely cancels out. Two parts in the same filament, in the same orientation and ideally on the same plate, shrink together and their patterns still match (Assemblies and tolerance stackups). The problem shows up against metal, bought parts or electronics. That is what decides when to compensate.

To separate scale from offset in a measurement you need two sizes, one of about 20 mm and another of 100 mm or more. The method and the arithmetic are in Parts that print the wrong size.

Shrinkage depends on direction

During extrusion the chains are stretched along the bead; as they cool they try to coil back up. That is why shrinkage is usually greater in the dominant bead direction. A long wall with its beads running lengthwise shrinks more along its length than across it. On parts with a dominant direction, measure X and Y separately. Do not expect, however, a round hole in an unfilled material to come out oval from shrinkage: an oval hole points to a mechanical problem on one axis, such as a slack belt or backlash.

Fiber-filled composites do the opposite: they shrink little along the bead, where the fibers dominate, and more across it.

Z is different. The nozzle sets each layer's height from the machine's Z position, so most of a layer's shrinkage happens before the next layer goes down, and it does not add up. After that, only the still-hot top keeps shrinking. In unfilled materials Z shrinkage is small and hard to measure, because heights come out in whole layers. Check the Z offset first. If your slicer has a field for Z, use it only with a tall measurement, 50–100 mm or more.

The first millimeter does not count: the base prints wide from elephant's foot, which is not shrinkage (The face on the bed). Take your measurements above it.

Measuring your filament's shrinkage

Print one part with a long dimension, 100 mm or more, in X and in Y, and another short one of about 20 mm to separate scale from offset. Use the same filament, profile, orientation, walls and infill as the real part. The long dimension matters: 0.3 % of 20 mm is 0.06 mm, the same as the repeatability of a hobby calliper; over 100 mm it is 0.3 mm.

Measure the part at room temperature, not straight off the plate. A PLA part still at 40 °C measures about 0.15 % long, half of what you are trying to measure. Measure nylon once it is conditioned, not as it comes off the plate, because it grows as it absorbs water.

The arithmetic fits on one line: s = (L_model − L_measured) / L_model. If 100 mm measures 99.6, s = 0.4 % and the scale factor is 1 / (1 − s) = 1.004. At these sizes it makes no difference whether you use 1/(1 − s) or 1 + s; they only diverge above a few percent, which is the case with sintering (Metal filaments and sintering).

Before you trust a number, check two spools of the same product: colors and batches vary. Factory profiles are a starting point, not your figure; an official profile can ship 0.18 % for a PC while your spools measure four times that. Write the result down next to the filament profile rather than relying on memory. The calibration parts and their order are in Dimensional calibration.

When to compensate, and where

Decide in this order:

  1. The part only mates with parts printed in the same filament and orientation. Do not compensate: the error cancels out.
  2. It mates with metal, a bought part, a circuit board or another family, or it has long functional dimensions. Compensate.
  3. The only thing failing is small holes. That is not shrinkage: Why holes print small.

For the borderline case, a rule of thumb: compensate when s × L exceeds roughly half the fit's clearance on diameter. With a sliding fit of 0.15–0.20 mm per side (0.3–0.4 mm on diameter) and 0.4 % shrinkage, that happens from about 40–50 mm of length. Below that length, the clearance absorbs it. The rule is conservative: the other half of the clearance is left for centering the part and for the machine's own error. Your machine's clearance values come from Real printed clearances.

Option A: the slicer's filament profile

The correction belongs to the material, so it goes in the filament profile: every part sliced with that filament gets it and the model stays at its nominal dimensions. As of late 2026, OrcaSlicer, Bambu Studio, PrusaSlicer and Cura all have the field, but with three different conventions, and the same number typed into the wrong slicer doubles the error. Parts that print the wrong size lists the field names and what each one expects.

There is a catch with multi-material: a slicer can only scale an object once. If an object mixes filaments with different shrinkage values, the slicer cannot apply each one's value at the same time, and depending on the slicer it applies only one or drops the compensation. Check the sliced dimensions or compensate in the model.

Option B: the model

Choose this option when the part will always be printed in the same material, or when the slicer cannot do it, as with multi-material. Do not scale the model of a standard part (a thread, a gear): leave its nominal dimensions and correct in the profile.

Compensate in one place only. If you enter the value in the slicer and also scale the model, you correct twice. And a scale does not replace the offset corrections (flow, XY compensation for contours and holes): those work in millimeters, not percentages.

After printing, the part keeps moving

diagram
Temperature and water change the size and give it back. Heat near Tg, late crystallization and sustained load change it for good.

Temperature, reversible

Plastic expands 5 to 8 times more per degree than steel (about 12 µm per meter per degree) and three to four times more than aluminum (about 23). Going from 20 to 50 °C, a 200 mm PLA cover bolted to an aluminum extrusion grows by about 0.4 mm; the aluminum, by about 0.14 mm. That 0.28 mm difference bows the cover or loads the bolts. The fix: one fixed hole as the datum and slots at the other end, or a fiber-filled filament, which expands much less along the bead. Service temperature limits are in Heat, cold, sunlight and chemicals.

Water, mostly reversible

Nylon grows as it absorbs water: PA6 more than PA12, PA11 or PAHT-CF. It takes weeks in a 2 mm wall and months in a 4 mm one. Design the fits for the conditioned part (Nylons and polyamides). In PLA, PETG, ABS or PC, moisture changes the print, not the size of the finished part (Drying and storing filament).

Heat near Tg, permanent

Printing leaves stresses frozen inside the part: stretched chains, layers that shrank against a hot bed. If the part gets close to its Tg, those stresses relax: it shrinks along the beads, grows in Z and bends if the stresses were uneven. That is why a PLA part on a car dashboard in summer or next to a window deforms long before it melts.

Two identical gray PLA car phone mounts side by side on a bench. The left one has a flat base and a straight clip arm. The right one spent a summer day on a dashboard: its base has bowed so the corners lift off the bench and the arm leans over, yet its edges, holes and layer lines are still crisp, with no sign of melting.
Two identical gray PLA car phone mounts side by side on a bench. The left one has a flat base and a straight clip arm. The right one spent a summer day on a dashboard: its base has bowed so the corners lift off the bench and the arm leans over, yet its edges, holes and layer lines are still crisp, with no sign of melting.

Annealing is the same effect done on purpose; its figures for dimensional change are in Annealing and strengthening.

Late crystallization, permanent

A semi-crystalline plastic printed cold can crystallize later if it is heated above its Tg, and when it does it shrinks again. It happens to PEEK printed with the chamber below about 120 °C that then runs hot, and to unannealed PLA-HT that goes above about 60 °C.

Sustained load, permanent

A part under constant load creeps: a press fit or a screw in a boss loses its grip over the weeks. The mechanism and how to design against it are in Creep and fatigue.

When it fails

Symptom, cause and fix
Symptom Cause Fix
The hole pattern does not line up with the plate's holes, but each hole fits Uncompensated shrinkage over a long dimension Measure your filament and correct it in the profile, or turn every hole in the pattern except one into a slot
You scaled to open up small holes and they are still tight That 0.1–0.3 mm comes from facets and the bulge on the curve, not from shrinkage Hole compensation or clearance in the design, not a scale
After compensating, everything comes out large Corrected twice (slicer and model) or with another slicer's convention Keep the correction in one place and check what the field expects
The measurement does not repeat between parts You measured hot, over 20 mm or on the elephant's foot Measure at room temperature, over 100 mm or more and above the first millimeter
After switching family, the fits are off Different shrinkage Print the clearance coupon again; within the same family, a check is enough
A nylon part that fitted on day one is tight weeks later It has taken on water and grown Design and measure fits on the conditioned part

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?