kapy academy

Carbon and glass fiber filaments

18 min readUpdated Nov 2026

A PLA bracket under a shelf bends more than it should. In PLA-CF it bends 30 % less: flexural modulus goes from 2.75 to 3.95 GPa on Bambu's datasheets. But it fails at almost the same load, without warning, and it splits between layers sooner: tensile strength in Z drops from 35 to 26 MPa. A short-fiber filament is its matrix plus stiffness. It is stronger only with some matrices, and then only in XY. It is more brittle. And it only takes much more heat when the matrix is semi-crystalline (PA, PET, PPA, PPS).

What is in the spool

Short carbon or glass fiber, chopped or milled, mixed into the molten plastic before the filament is extruded. Each fiber is a few microns across (about 7 µm for carbon; 10–15 µm for glass). Compounding and filament extrusion break it up further, and in the spool it ends up of the order of tenths of a millimeter long.

Fiber content usually sits between 10 and 30 %. Some brands put it in the name: in Polymaker's Fiberon range, the number in PA12-CF10, PA612-CF15, PA6-CF20 or PA6-GF25 is the fiber content according to the maker. Many spools do not say; the datasheet only lists "carbon fiber" in the composition.

Carbon fiber has a modulus of about 230 GPa, glass fiber 70–75 GPa. The matrix stays at 2–3 GPa. With those figures you would expect far stiffer parts; yet common desktop composites top out around 10 GPa (Bambu's PPA-CF gives 9.9). Much of the reason lies in how load gets into a short fiber. The fiber is not gripped at its ends: the matrix drags it by shear along its surface. Stress inside the fiber starts at zero at each tip and builds toward the middle. If the fiber is shorter than the critical length, often a few tenths of a millimeter in thermoplastics, the stress never reaches the fiber's strength: before that, the interface with the matrix gives way and the fiber pulls out. At small strains the matrix transfers load well and the fiber stiffens the part. At large strains the interface lets go and the fiber stops helping.

tensionshort fiberfiber pulled outcrack at the tipstress in the fibercritical lengthtensionlong or continuous fiberstress in the fiber
Load enters the fiber by shear and builds from zero at each tip. A fiber shorter than the critical length pulls out of the matrix before it breaks; a continuous one carries load at full stress.

Other causes add to this. Every fiber tip is a notch: a point where stress concentrates and a crack can start. With thousands of tips per cubic millimeter, elongation at break and toughness go down. Fiber-filled beads trap more microvoids than the neat matrix. And the bond between fiber and matrix depends on the fiber's surface treatment, which every maker handles its own way. That is why short fiber raises stiffness a lot and strength little or not at all.

The nozzle aligns the fiber with the bead

As it enters the nozzle cone, the molten plastic speeds up. That converging flow rotates the fibers into line with it, and they come out lying along the path. A fiber-filled part is only a composite along each bead.

A printed part behaves differently in three directions:

  • Along the bead. The fibers do the work. This is the XY value on the datasheet.
  • Between neighboring beads in the same layer. Almost no fiber crosses the weld between beads: the matrix is in charge there, and the bond is weaker.
  • Between layers, in Z. No fiber crosses the layer bond, and the fibers sitting on the bead surface reduce the area of plastic that welds to the next layer. This is the worst direction.
Section through a nozzle laying a bead of fiber-filled filament on the layer below: in the melt in the barrel the short fibers tumble, the cone turns them along the flow and they come out lying along the bead, as in the layer below; none crosses the weld between the two layers
The nozzle cone turns the fibers along the flow. Inside each bead they run parallel to it, and none crosses the weld to the neighboring bead or to the layer below: only plastic is there. A schematic, not to scale: real fibers are tenths of a millimeter long and a few microns thick.

The datasheets bear this out. On Bambu's (revision V2.0 for the base materials), the share of XY strength kept in Z drops when fiber is added: PLA keeps 90 % (35 of 39 MPa) and PLA-CF 68 % (26 of 38); PETG keeps 81 % (39 of 48), and PETG-CF 64 % (38 of 59). ABS-GF is the exception: it keeps 81 % (29 of 36), not because it improves in Z, but because the fiber lowers its XY strength, from 41 to 36 MPa. Semi-crystalline composites keep the least: PAHT-CF 51 %, PET-CF 47 %, PA6-GF 36 %, PPA-CF 34 %, PPS-CF 28 %. Stiffness follows the same pattern: PLA-CF gives 3.95 GPa in flexure in XY and 2.26 in Z, less than unfilled PLA in Z (2.37); PET-CF, 5.3 and 2.2; PPA-CF, 9.9 and 3.2.

For design, assume the part is half as strong in Z as in XY, or 30 % if the material is fiber-filled, and orient it so the main load runs along the beads (Layer adhesion and anisotropy). Walls follow the part's outline, so the outline is where the fiber runs, and a bracket gets its stiffness from its walls more than from its infill.

Shrinkage depends on direction too. Along the bead it is about 0.2–0.5 %, because the fiber does not shrink and holds the matrix back; across beads and in Z it is larger. So a long, straight fiber-filled wall warps less than one in the neat matrix, but the part can bow or go oval where the beads change direction. Holes and fits still call for a calibration coupon (Shrinkage and dimensional stability).

What the part gains and loses

The fair comparison is between a base material and its fiber-filled version from the same maker, measured with the same tests on the same printer. These are the XY values from Bambu's datasheets (V2.0 for the bases, V1.0–V2.0 for the filled versions). V3.0 of PLA Basic and PETG Basic gives different figures, so do not mix them with these.

Base versus fiber-filled, same maker (Bambu datasheets, XY)
Pair Flexural modulus (GPa) Tensile (MPa) Elongation at break (%)
PLA → PLA-CF 2.75 → 3.95 (×1.4) 39 → 38 12.2 → 8.4
PETG → PETG-CF 1.79 → 2.89 (×1.6) 48 → 59 11.2 → 10.4
ABS → ABS-GF 1.88 → 2.86 (×1.5) 41 → 36 10.5 → 6.3
ASA → ASA-CF 1.92 → 3.74 (×1.9) 52 → 34 9.2 → 9.6

Stiffness rises by 44 to 95 % in every pair. Strength stays within a few MPa of the base, or drops: ASA-CF loses 35 % against ASA. Elongation drops or barely moves. In consumer matrices, "carbon fiber" on the label means more stiffness and a better finish, not more strength. PETG-CF is the exception: it gains 23 % in XY strength (from 48 to 59 MPa) and keeps almost all of PETG's ductility. That makes it the most sensible composite to start with. In nylon and PET with well-bonded fiber, XY strength also rises (PAHT-CF gives 92 MPa), but in Z it stays at half or less.

unfilledfiber-filledPLA / PLA-CFPETG / PETG-CFABS / ABS-GFASA / ASA-CFflexural modulus XY (GPa)2.753.951.792.891.882.861.923.74tensile XY (MPa)3938485941365234elongation at break XY (%)12.28.411.210.410.56.39.29.6HDT at 0.45 MPa (°C)575569748799100110205PET-CF (semi-crystalline)
Four pairs from one maker: fiber raises stiffness by 44 to 95 %; strength barely changes or drops, except in PETG-CF; elongation drops or stays put, and the HDT of amorphous matrices hardly moves. With a semi-crystalline matrix, such as PET-CF's, it shoots up.

Failure is brittle. A fiber-filled part does not yield before it breaks: it does not bend, it does not whiten, it gives no warning. A clip, a snap-fit or a part that will get dropped calls for the unfilled matrix. Charpy impact values from printed specimens are no use for comparing makers or predicting a snap fit; the reason is in Stiffness, strength and toughness, and the snap-fit math in Print-friendly snap fits.

Fiber does help against creep: along the bead, the fibers carry the sustained load under which the neat matrix would slowly deform. A part loaded for months deforms less (Creep and fatigue).

The matrix sets the temperature

After "stronger", the most common mistake is believing the fiber raises the temperature the part can take. With an amorphous matrix, it barely does: −2 to +12 °C. HDT at 0.45 MPa, on the same maker's sheets: PLA 57 °C, PLA-CF 55 °C; PETG 69, PETG-CF 74; ABS 87, ABS-GF 99; ASA 100, ASA-CF 110. A PLA-CF part sags in a car in the sun like a PLA one.

With a semi-crystalline matrix, the jump is huge: PA6-CF 186 °C, PA6-GF 182, PAHT-CF 194, PET-CF 205, PPA-CF 227, PPS-CF 264. Unfilled nylon stays at 90–130 °C.

The physics is the same in both families. Above its glass transition (Tg), an amorphous polymer turns rubbery all the way through. Short fibers cannot hold up a rubber, so the specimen gives way near Tg: PETG-CF has a Tg of 68 °C and an HDT of 74. In a semi-crystalline polymer, the crystals stay solid up to the melt and form a network. Above Tg only the amorphous part softens. The fibers stiffen that network enough to pass the lenient 0.45 MPa test far above Tg: PET-CF has a Tg of 75 °C and an HDT of 205 °C.

Those high figures come from annealed, dry specimens: the PAHT-CF sheet states they were annealed and dried at 80 °C for 12 h before testing. Crystallinity depends on how the part cooled, and a part fresh off the bed in a lukewarm chamber can end up far less crystalline. A heated chamber helps during the print and annealing finishes the job: Bambu gives 80 to 130 °C for several hours for its PA and PET composites (6 to 12 on the PAHT-CF sheet), and warns that the part may distort in the oven. If the part will run hot, anneal it. The procedure is in Annealing and strengthening.

In summer, a car's dashboard in the sun reaches 70–100 °C. A loaded part there needs a fiber-filled compound: PA-CF, PET-CF or PPA-CF. Unloaded or in the shade, in the console or the glovebox, ASA, PC or annealed PLA-HT will do, and PC wherever it takes knocks. Inside a car, never PLA or PETG, and not PLA-CF or PETG-CF either: the matrix is the same. Next to an engine, stick with PET-CF, PA-CF, PAHT-CF or PPA-CF, annealed.

Carbon or glass

Carbon fiber is about three times stiffer than glass, so with the same matrix the part comes out stiffer. It is also less dense (about 1.8 g/cm³ against about 2.5 for glass), and the part weighs less. It is always black or very dark and leaves a deep matt finish.

Glass fiber is less stiff and usually cheaper. It is an electrical insulator and does not block radio signals, so it suits electronics housings and antenna covers. It takes color: Bambu's ABS-GF and PA6-GF come in several colors.

Although carbon fiber conducts a little, a CF part is not reliable as anti-static or conductive. For protection against electrostatic discharge there are filaments with certified resistivity, in Functional specialty filaments. Both fibers are abrasive and both need a hardened nozzle.

Matrix by matrix

Common composites: starting values (Bambu datasheets)
Material Flexural modulus XY HDT at 0.45 MPa Good for Watch out for
PLA-CF 3.95 GPa 55 °C jigs, drone frames, stiff display parts at room temperature, matt look heat; it is brittle
PETG-CF 2.9 GPa 74 °C stiff general-purpose jigs and brackets; the default composite load above ~55 °C
ABS-GF / ASA-CF 2.9 / 3.7 GPa 99 / 110 °C stiffer, lower-warp ABS or ASA, housings and outdoor parts (ASA) ASA-CF is weaker than ASA
PA-CF / PAHT-CF 4.2 GPa (PAHT-CF) 186 / 194 °C the go-to functional composite: tooling, mounts near engines, gears that must not deform when hot drying and chamber; dry values
PET-CF 5.3 GPa 205 °C the stiffest common composite; takes up little water (0.37 %), stable in damp places chamber; brittle (4.5 % elongation)
PPA-CF / PPS-CF 9.9 GPa (PPA-CF) 227 / 264 °C under the bonnet, chemical contact hotend of 300 °C or more (PPA-CF) or 320–350 °C (PPS-CF), and a heated chamber

The fiber-filled nylon values are for dry specimens. Once the part takes up moisture from the air, modulus and HDT drop noticeably; how to design for the conditioned part is in Nylons and polyamides. PC-CF and PC-GF follow the logic of amorphous matrices: the fiber gives PC stiffness, not more temperature (Polycarbonate and its blends). The step above PPA-CF and PPS-CF is in PPS, PEEK, PEKK and PEI.

Rough prices as of late 2026: PLA-CF and PETG-CF, €30–50/kg; PA-CF and PAHT-CF, €55–110; PET-CF, €60–100; PPA-CF, €150–210. The comparison across every family is in Filament comparison table. Besides Bambu's, there are composites from Polymaker (Fiberon range), Prusament and other brands; always read the datasheet for your spool.

What the printer needs

Nozzle

With abrasive fillers use a hardened nozzle, preferably 0.6; hardened steel needs 5–10 °C more or 10–20 % less flow (Nozzles: size and material). With fiber, never 0.2, and never brass or stainless steel, for two physical reasons. The first is abrasion: a few hundred grams of fiber-filled filament visibly widen a 0.4 mm brass nozzle, the bead comes out wider and every dimension shifts: thicker walls, smaller holes, tighter clearances. Hardened steel wears too, but in kilos. The second is clogging: in a small orifice the fibers jam against each other and plug it.

Speed, extruder and switcher

Makers set lower speeds for composites than for the neat matrix: on Bambu's sheets, PETG-CF below 200 mm/s and PET-CF below 100 mm/s. Fiber-filled melt flows worse and a hardened nozzle melts less plastic per second. Start from the maker's profile.

The extruder gears wear as well. If you print composites often, swap them for hardened ones (Extruders: direct drive or Bowden).

Fiber-filled filament is brittle: it snaps on tight bends or under the cutter, and it also wears the feed parts and PTFE tubes. Before loading it into an AMS, MMU or CFS, check that the material is on the maker's supported list (Filament switchers: AMS, MMU, CFS and ACE).

Drying, chamber and bed

Drying, chamber and bed settings follow the matrix:

Printing and drying composites (starting values)
Material Nozzle (°C) Bed (°C) Chamber Drying
PLA-CF 210–240 45–65 no; part fan at 100 % same as PLA
PETG-CF 240–270 65–75 35–50 °C (datasheet) 65 °C × 8 h
ABS-GF / ASA-CF same as ABS / ASA same as ABS / ASA enclosed printer 75–80 °C × 8 h
PA-CF / PAHT-CF 260–300 80–120 heated, recommended 85 °C × 12 h, mandatory
PET-CF 260–300 80–120 heated, recommended 80 °C × 8–12 h, mandatory
PPA-CF 285–320 100–120 heated 100–140 °C × 8–12 h in an oven

PA-CF and PET-CF print with the part fan at 0–30 % and glue on PEI. The stock hotend on current machines (290–300 °C) is enough for both; PPA-CF needs at least 300 °C (285–320 °C) and PPS-CF a 320–350 °C hotend, such as the one on the Bambu X1E (320 °C) or the H2 series (350 °C). More in Drying and storing filament and Enclosures and heated chambers. For PA-CF and PET-CF parts there are dedicated support interface materials, in Support materials.

Finish, sanding and dust

Fibers near the surface break up the polymer's smooth skin, so light scatters instead of reflecting as it would off a mirror. The result is a matt finish that hides layer lines. For visible parts it is a real advantage, but it hides the lines from the eye, not their weakness.

Continuous fiber: a different technology

Some printers lay a continuous tow of carbon, glass or aramid fiber inside the part: some through a dedicated nozzle next to the plastic one, others impregnated with plastic inside the bead. These are machines such as Markforged's Mark Two and FX range, Anisoprint's, or the FibreSeeker 3, announced in 2025 for the desktop. Along the laid fiber, stiffness and strength sit far above any short-fiber filament, because the fiber is never shorter than the critical length. But they only reinforce where the slicer places the fiber, they stay weak in Z, and they need a dedicated machine and dedicated software. If your part needs that, see When to order the part instead.

When it fails

Common symptoms with fiber-filled filaments
Symptom Cause Fix
The clip or snap-fit breaks the first time it is used The fiber cuts elongation (ABS 10.5 % → ABS-GF 6.3 %) Unfilled matrix: PETG, PA or PC
The bracket is stiff but splits along a layer line Z keeps ~30 % of the XY strength Reorient so the load runs along the beads
After a few spools, holes come out smaller and outside dimensions larger Worn brass or other soft nozzle 0.6 hardened nozzle, then recalibrate
Clogs or under-extrusion with a 0.4 nozzle Fibers jam in the orifice; the hardened nozzle melts less 0.6 nozzle, more temperature or less speed
A PLA-CF or PETG-CF part deforms somewhere warm Amorphous matrix: HDT of 55 and 74 °C PET-CF or PA-CF, annealed
A PA-CF part takes less heat than expected Printed without annealing, low crystallinity Heated chamber and annealing
The filament snaps in the switcher or along the path Brittle composite and tight bends Straighter path, dry filament, maker's list
A PA-CF part warps or comes out rough and stringy Wet filament or no chamber Dry at 85 °C × 12 h and print enclosed
The part breaks below the datasheet value The sheet gives XY values on ideal specimens Design with Z at 30 % and test a coupon (Estimating whether a part will hold)

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?