Use nylon for parts that turn, rub or take knocks for months: a gear, a bushing, a clip that hits the floor every week, a hook soaked in oil. That is nylon's territory: it resists wear, repeated impact and oil better than any other common filament. It has one catch that no other common family shares: its properties change with the humidity of the air, because it absorbs water and that water stays inside the part. Filled or not, design for a part that keeps changing after it leaves the printer.

What the numbers mean: PA6, PA12, PAHT, PPA

Polyamide (PA) is a family, not a single material. The number counts the carbon atoms in each repeating unit of the chain; in the two-number grades, such as PA66 or PA612, the first is the diamine's and the second the diacid's. Between one unit and the next sits an amide group, which ties neighboring chains together through hydrogen bonds. In PA6 the amide groups are close together. In PA12 and PA11 they are far apart. PA612 sits in between.

PA6PA12many amide groupsstiffer and higher-meltingwhen dry, absorbs more waterfew amide groupssofter, melts lower, absorbs little wateramide grouphydrogen bondwater
Amide groups tie the chains together, and they are also where water latches on. How densely they sit along the chain decides how each polyamide behaves.

That spacing explains almost everything, because the amide groups are where water molecules attach. More amide groups: more water absorbed, a higher melting point, and a stiffer, stronger part when dry. Fewer amide groups: less water, a lower melting point, and a softer, more stable material.

  • PA6: the stiffest and strongest when dry, and the one that absorbs the most water. As injection-molded resin it takes on 2.5–3 % at 50 % relative humidity and close to 9 % at saturation.
  • PA12 and PA11: as injection-molded resin, 0.5–1 % at 50 % humidity and around 1.5 % at saturation. They print cooler, at the low end of the 250–290 °C range, and they change the least with humidity. They are also softer.
  • Copolymers (CoPA): many unfilled filaments are PA6/PA66 copolymers. Polymaker's PolyMide CoPA, for example, has its glass transition (Tg) at 66 °C and melts at 189 °C. In water uptake it behaves far more like PA6 than PA12. Unfilled PA612 or PA12 filaments are scarce.

PAHT is a trade name, not a chemistry. According to its datasheet, Bambu Lab's PAHT-CF is PA12 blended with other long-chain polyamides and carbon fiber. Its selling point is low water uptake (0.88 % at 25 °C and 55 % humidity), and it reaches an HDT of 194 °C at 0.45 MPa thanks to the fiber and the crystallinity. Read the composition line on the datasheet, not the acronym: Reading a material datasheet shows where to find it.

PPA (polyphthalamide) is a semi-aromatic polyamide: the rings in its chain raise heat resistance and cut water uptake. It is sold filled, as PPA-CF or PPA-GF; PPA-CF gives an HDT of 227 °C at 0.45 MPa. It wants a 285–320 °C nozzle, so you need a hotend that reaches 320–350 °C and a heated chamber.

If you do not need to print the nylon part yourself, note that powder-sintered PA12 and PA11 (SLS or MJF) are the most common printed nylon parts in service: nearly isotropic and free of warping. When to order the part instead explains when that pays off.

Water is part of the material

Water causes two different problems, and it pays to keep them apart.

The first is a printing problem: wet filament prints badly, because the water boils in the nozzle and degrades the polymer. Drying fixes it; the procedure is in Drying and storing filament.

The second is a design problem, and it is the one that matters here: the printed part absorbs water from the air while in use, and its properties change. Water molecules slip in between the chains, right at the amide groups, and break some of the hydrogen bonds holding them together. The chains slide past each other more freely. The part becomes softer, weaker and much tougher, and its Tg drops. The water acts as a plasticizer, the role additives play in flexible PVC.

The PolyMide CoPA datasheet measures both states with the same test, so the figures are comparable:

PolyMide CoPA: dry versus wet (Polymaker datasheet)
Property (XY unless stated) Dry Wet
Young's modulus 2.70 GPa 0.72 GPa
Tensile strength 78 MPa 34 MPa
Tensile strength in Z 45.8 MPa 13.7 MPa
Notched Charpy impact 6.9 kJ/m² 27.7 kJ/m²
0 %100 %200 %300 %400 %100 %27 %stiffness100 %44 %strength100 %400 %toughnessdrywet
Each group is normalized to its dry value. Data from Polymaker's PolyMide CoPA datasheet.

The wet column is the extreme case. According to the same datasheet, at 23 °C and 70 % humidity CoPA reaches 2.8 % water after about six weeks; at 50 % it will settle somewhat lower. Its properties then sit somewhere between the two columns, and nobody publishes exactly where.

Hence the design rule: base stiffness and strength on the conditioned values, those of a part that has reached equilibrium with the ambient humidity. If the datasheet gives only dry values, which is the usual case, expect to lose a good share of the stiffness and strength (Estimating whether a part will hold). The gain in toughness, on the other hand, only shows up once the part is conditioned.

Chemistry and fiber soften the effect. According to Bambu, its older PA-CF loses 40–45 % of its mechanical properties when it absorbs water, and the long-chain PAHT-CF only 12–18 %. That is a manufacturer's figure with no published protocol: treat it as an order of magnitude.

PA6-GFPA6-CFPA-CF (older grade)PPA-CFPAHT-CF0 %1 %2 %3 %equilibrium water, 25 °C / 55 % RH
Equilibrium water uptake at 25 °C and 55 % humidity, from one manufacturer's datasheets so the bars are comparable. The chain chemistry nearly triples the figure.

How long does it take? Longer than you would think. Water gets in by diffusion, and the time grows with the square of the thickness: in room air, a 2 mm wall takes weeks to reach equilibrium and a 4 mm wall takes months. The porosity between the beads of a printed part shortens that, but not to days.

The dimensions change too: the part grows as it absorbs water, more in PA6 than in PA12. On a gear or a bushing, leave a little extra clearance for it. Measure fits and coupons on the conditioned part, not straight off the plate; Iterate and measure and Test coupons explain how.

Dry or conditioned: when to test the part

Freshly printed nylon is at its stiffest and most brittle. Dry CoPA gives 6.9 kJ/m² of notched Charpy impact, a quarter of its wet value. A clip that snaps on day one may work a few weeks later, once it has taken on water.

For snap fits and parts that flex, design to the allowable strain of conditioned nylon: 6 % if it is assembled once, and 4 % if it is assembled and taken apart often. Do not test them the day you print them: dry nylon is far less forgiving (Print-friendly snap fits).

You can speed up conditioning by soaking the part in warm water for a day or two. It comes out holding a lot of water and then gives some back to the air until it reaches equilibrium with the room. That is enough to check toughness, but measure fits once the part has stabilized. There is no standard recipe; this is shop practice. Never boil a part that has to keep its fits.

Annealing works with nylon too, because it is semicrystalline. The PAHT-CF datasheet suggests 80 to 130 °C for 6–12 h; Polymaker suggests 80 °C for 6 h for CoPA. It raises stiffness and heat resistance and relieves internal stresses. The risk: the part can distort in the oven. The method is in Annealing and strengthening.

Why HDT misleads with nylon

Nylon is semicrystalline and has a low glass transition: around 40–70 °C when dry (PA12 at the low end, 66 °C for CoPA, 70 °C for PAHT-CF), and lower once wet. Above Tg the amorphous phase turns rubbery while the crystals hold the shape. That is why, under the light 0.45 MPa load, the test bar does not reach the specified deflection until 90–130 °C, even though its stiffness has already fallen to a fraction of its room-temperature value.

One datasheet is enough to see it: CoPA gives 111 °C at 0.45 MPa and 70 °C at 1.8 MPa, practically its Tg. An amorphous plastic barely separates the two figures: Bambu's PLA Basic gives 57 and 54 °C. The further apart the two HDTs, the more the 0.45 MPa figure overstates what a loaded part will take.

For a part under sustained load in the heat, such as a motor mount or something inside a car, unfilled nylon does no better than ABS or ASA. Look at HDT at 1.8 MPa and keep a 15–20 °C margin below it (Heat, cold, sunlight and chemicals), or move to a fiber-filled grade. At 0.45 MPa the filled grades give 186 °C (PA6-CF), 194 °C (PAHT-CF) and 227 °C (PPA-CF); PAHT-CF holds 170 °C at 1.8 MPa, which means about 150 °C under load.

Unfilled nylon also creeps under constant load, more so when wet and warm. A shelf bracket or a clamp that has to keep its grip calls for a fiber-filled grade or PC. Creep and fatigue explains why.

Where nylon wins

Wear and sliding. Nylon has low friction and wears slowly against steel and against itself: gears, bushings, slides, cams, hinge pins. That is why Spur gears recommends polyamide for continuous torque. Plain nylon is not self-lubricating; the self-lubricating grades carry PTFE or MoS2. Under high load and speed, friction heats it and softens it: limit the speed or lubricate. Seating bearings and bushings explains when a bronze bushing or a bearing is worth it. Fiber-filled grades hold the tooth shape better in the heat, but exposed fiber can wear down a softer gear running against them. There is no reliable data for printed gear pairs: test yours.

Impact and fatigue. Once conditioned, nylon survives drops and repeated flexing that crack PLA: tool handles, clips, brackets that take knocks.

Chemicals. It resists oils, greases and fuels. The PAHT-CF datasheet confirms this and adds that it does not resist acids, alkalis or some organic solvents. The full tables are in Heat, cold, sunlight and chemicals.

Where nylon loses

  • Rigid brackets and housings. Unfilled, its dry modulus runs from 1 to 2.7 GPa depending on the grade; the best CoPA comes close to PLA's 2.8 GPa, but conditioned it drops to a fraction of that (0.72 GPa on its datasheet). Only fiber-filled grades are stiff in service. Stiffness, strength and toughness explains why.
  • Precise fits that must not shift with the seasons. Use PETG, ASA or a long-chain fiber-filled grade.
  • High-cycle living hinges. As a 180° folding hinge it breaks within a few hundred folds, like every rigid plastic in the test in Living hinges and flexures, although it is the best of them. As a flexure working below 4 % strain it holds up fine. For hinges, the material is polypropylene; see Polypropylene.
  • Outdoors, in the sun. Unless it carries a UV stabilizer or black pigment, test it before you leave it in the sun; aging is covered in Heat, cold, sunlight and chemicals.

Printing unfilled nylon

Unfilled PA6, PA12 and PA11: starting values
Parameter Value
Nozzle 250–290 °C (PA12 and PA11 at the low end)
Bed 90–120 °C
Enclosure passive or heated chamber
Fan 0–30 %
Surface glue stick on PEI, or garolite (G10)
Nozzle material brass (fine)
Drying 80–85 °C × 8–12 h, mandatory

These ranges are for generic PA6 and PA12. Some copolymers sold as "warp-free" ask for something else: Polymaker's CoPA wants the bed at 25–50 °C on PC or textured PEI, the fan off, an enclosure, and drying at 100 °C for 8 h. Follow the datasheet for your spool.

Why it lifts. Semicrystalline polymers shrink more as they cool because the chains pack into crystals: 1–2 % linear against PLA's 0.2–0.5 %. Each layer pulls on the one below, which is already cooler; corners lift and tall parts split between layers. Hence the enclosure and the glue or garolite. The list of remedies is in Warping and lifting corners.

Drying. Dry at 80–85 °C for 8–12 h and print from the dryer or a dry box; Bambu and Polymaker ask for under 20 % relative humidity for storage and printing. A freshly dried spool left in the open is wet again the same day. A 65 °C dryer, such as the AMS 2 Pro's, is not enough for nylon; an 85 °C one, such as the AMS HT's, is. Do not exceed the datasheet temperature or leave the spool in the dryer for days: nylon oxidizes, yellows and turns brittle. The signs of wet filament are popping, steam, stringing, a matt, rough surface and weak layers.

Fits. With 1–2 % shrinkage, a Ø20 mm hole comes out roughly 0.1–0.35 mm tighter than in PLA. Reprint the clearance coupon and measure it after conditioning (Real printed clearances, Shrinkage and dimensional stability).

Fumes. Nylon emits caprolactam, between 2 and 180 µg/min, plus ultrafine particles. Print with an enclosure and a HEPA plus activated-carbon filter, or with extraction to outside, and never in a bedroom (Emissions and ventilation).

Heat-set inserts. Set the iron to 280–300 °C and make sure the part is dry; otherwise the plastic around the insert bubbles (Designing for heat-set inserts).

Why nearly all nylon is fiber-filled

Short carbon or glass fiber solves three problems.

  1. It cuts shrinkage along the bead to 0.2–0.5 %. The fibers do not shrink and they hold the matrix, so warping drops so far that filled grades rate as easier to print than unfilled nylon: difficulty 3 against 4 in the Filament comparison table.
  2. It multiplies stiffness and raises HDT. PAHT-CF gives a flexural modulus of 4.2 GPa in XY, several times that of a conditioned unfilled nylon, and filled grades reach an HDT of 186–227 °C at 0.45 MPa.
  3. It dilutes the polymer, so the part absorbs less water and loses less as it conditions.

In exchange you lose toughness and elongation: PAHT-CF breaks at 8.4 % in XY and PA6-GF at 3.9 %. Strength in Z falls by half (47 MPa against 92 in XY for PAHT-CF), and when designing, be more cautious than the datasheet: assume the part is 30 % as strong in Z as in XY. With abrasive fillers use a hardened nozzle, preferably 0.6 (Nozzles: size and material); never 0.2 mm, brass or stainless steel. It also costs more: €55–110/kg for PA-CF or PAHT-CF against €40–80/kg for unfilled nylon (indicative prices at the end of 2026).

Fiber-filled nylon: starting values
Material Nozzle Bed Chamber Fan Drying
PA-CF/GF, PAHT-CF 260–300 °C 80–120 °C heated recommended (45–60 °C per the PAHT-CF datasheet) 0–30 % 85 °C × 12 h
PPA-CF/GF 285–320 °C 100–120 °C heated 0–20 % 100–140 °C × 8–12 h, in an oven

All of them want a hardened nozzle and glue stick on PEI or on a textured engineering plate.

Carbon or glass? Glass gives somewhat less stiffness, somewhat more toughness and does not conduct electricity; carbon is stiffer and always black. The rest is in Carbon and glass fiber filaments.

Which nylon for which part

Which polyamide for which job
Use Material Why
Gears, bushings, slides indoors and dry unfilled PA12 or CoPA low wear, toughness
Clips, handles, parts that get dropped unfilled CoPA or PA6, conditioned highest toughness once conditioned
Jigs, fixtures and rigid brackets near a motor PAHT-CF or PA12-CF stiffness and HDT from the fiber
Damp or outdoor service with stable dimensions long-chain PA (PA12, PAHT) absorbs and changes far less than PA6
Under the bonnet, under load PAHT-CF up to about 150 °C; PPA-CF above that HDT at 1.8 MPa and a 15–20 °C margin

Above PPA-CF come the materials in PPS, PEEK, PEKK and PEI. If you need toughness, stiffness and stable dimensions all at once in a damp or hot environment, look at Polycarbonate and its blends.

Examples on the market include Bambu Lab's PA6-CF, PA6-GF, PAHT-CF and PPA-CF, and Polymaker's Fiberon range (PA6-CF20, PA6-GF25, PA612-CF15, PA12-CF10) alongside its PolyMide CoPA.

As for the printer: unfilled nylon and PA-CF print on a modern stock hotend (290–300 °C) in an enclosed CoreXY. An open bedslinger handles small CoPA or PA-CF parts, but large unfilled nylon parts warp. PPA-CF wants a 320–350 °C hotend and a heated chamber: machines such as the Bambu X1E (320 °C) or the H2D and H2S (350 °C). The differences between a passive enclosure and a heated chamber are in Enclosures and heated chambers.

When it fails

Symptom, cause and fix
Symptom Cause Fix
Popping, steam, stringing, matt and rough surface wet filament dry at 80–85 °C × 8–12 h and print from the dryer
Corners lift or the part comes loose from the plate 1–2 % shrinkage with no enclosure or no glue enclosure, glue stick on PEI or garolite, a brim; or move to a filled grade
The clip snaps the first time and works weeks later tested dry condition it in water before testing; design to the conditioned strain
Perfect fit on day one, tight weeks later the part grows as it absorbs water measure after conditioning; increase the clearance
A bracket sags in the heat Tg below the service temperature, creep filled grade or PC; check HDT at 1.8 MPa
The part welds itself to the plate and will not come off nylon grips some surfaces far too hard glue stick as a release agent, or garolite
The brass nozzle's bore widens after a few spools of PA-CF abrasive fiber hardened nozzle

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?