kapy academy

Flow ratio and max flow tests

16 min readUpdated Nov 2026

If a new brand of PLA gives top surfaces with fine ridges and a pin that used to fit now grips, it is the flow: that spool lays down slightly more plastic than the profile expects. If a fast profile gives a glossy outer wall with thin, matt infill behind it, it is the melting ceiling. These are two numbers with different tests. The flow ratio is a correction factor, close to 1, that scales the volume of every bead. The maximum volumetric flow is a ceiling in mm³/s that the slicer respects by slowing down.

Before you print anything

Both tests measure the filament under specific conditions. Pin them down first, or you will be measuring something else.

  • Dry filament. Wet filament foams in the nozzle and under-extrudes, so the test would measure the water. Dry it first (Drying and storing filament).
  • Temperature already chosen with the tower. Temperature changes viscosity, so it moves the real flow a little and the maximum flow a lot. Tower first (Temperature towers and retraction tests), then these tests.
  • The nozzle, plate and printer profile you will print with. A different nozzle (0.6 mm, hardened steel, high flow) means repeating the tests, especially the max flow test.
  • The right filament profile selected. Orca's test adds its correction to the current flow of that profile. If another one is selected, you are correcting the wrong value.

On a machine with two nozzles or a toolchanger, run both tests per nozzle. If one is hardened or high flow, its numbers differ, and each gets its own profile or its own per-nozzle value.

Calibrate in three rounds: the machine once, then each filament (temperature, flow, maximum volumetric flow, pressure advance) and the part's dimensions last (What to calibrate, and in what order).

Correct each error in one place only. The flow ratio absorbs everything that makes the real volume differ from the calculated one for that filament: its average diameter, how hard the drive gear bites (a soft filament and a hard one advance differently per motor turn) and the material itself. That is why the diameter field stays at 1.75 even if your spool measures 1.73. The difference is (1.73/1.75)² ≈ 0.977, 2.3 % less plastic, which the flow test already captures. Change the diameter as well and you correct the same error twice (What comes on a spool of filament). Do not touch E-steps or rotation_distance to fix a filament either: they are a constant of the gear train, calibrated once when the extruder is assembled (Extruders: direct drive or Bowden). And do not add a flow percentage in the firmware (M221) or on the printer's screen on top of it: that multiplies the slicer's value and nobody remembers it is there.

Why you read it on the top surface

The slicer lays the top-surface lines at a fixed spacing, set by the line width (around 0.45 mm with a 0.4 mm nozzle; 0.42 in Bambu Studio) and the overlap it calculates. The volume of each bead is fixed, and so is the space it has to fit in. Surplus plastic can only go up and sideways: ridges the nozzle drags on the next pass, a rough feel, a mark at the end of each line. Too little leaves grooves and, at worst, gaps you can see the infill through. At the right value the beads touch and close up: a flat surface that reflects light evenly.

Low flow (0.95)Correct flow (1.00)High flow (1.05)groovegapflat surfacefixed spacingridgedragWall measured with calliperscallipers rest on the ridges0.01 mm ≈ 2 % of a 0.45 mm bead
With the spacing fixed, flow decides whether the beads leave grooves, close into a flat surface or raise ridges the nozzle drags. Callipers rest on the ridges: their error is as large as the correction.

Measuring a single-bead wall with callipers, the classic method, is no longer recommended. A wall does not measure exactly n × line width: the slicer's bead model and the overlap between walls change it. The jaws rest on the layer ridges, not on the mid-plane. And the measuring error is as large as the correction you are after: 0.01 mm on a 0.45 mm bead is 2.2 %, and a typical correction is a few percent. A top surface sums thousands of beads and makes a 1–2 % difference visible to the naked eye.

What the top surface does not tell you is whether the part comes out the right size. Dimensional calibration tells you that, and it comes later (Dimensional calibration). Do not tune the flow ratio to make a cube measure 20.00 mm: you would be loading shrinkage and contour offset onto the flow ratio, and the error would come back on every other part.

The flow test in Orca

It is under Calibration › Flow rate. The method Orca's guide recommends is YOLO: a single plate with 11 blocks, whose modifiers run from −0.05 to +0.05 in steps of 0.01 and are added to the profile's current flow ratio. If your profile has 0.98 and the best block is +0.01, the new value is 0.99. In current Orca versions the top surface of each block uses an "Archimedean chords" pattern. The inner spiral prints last, and the line where it meets the arcs gives away whether material is piling up.

−0.05−0.04−0.03−0.02−0.010+0.01+0.02+0.03+0.04+0.05Modifiergaps between arcsmaterial piled up at the spiralbest blocksmooth surfaceno gaps between arcsspiral mark barely visiblenew = current + modifierbest at an end → repeat around it
On the YOLO plate, flow rises from left to right. You pick the smooth block with no gaps and the faintest spiral mark; if the best one sits at an end, the real value is outside the range.

Read it under raking light (a low lamp, from the side) and run a fingernail across it. Look for the smoothest block, with no gaps between the arcs and the faintest contact line between spiral and arcs. In the example in Orca's guide, +0.01 is chosen even though that line is still faintly visible, because gaps open up below it. Between two near-identical blocks, take the higher one if the lower one shows any gap: gaps weaken the top skin and let water in (Top surfaces).

If the best block is at an end, −0.05 or +0.05, the right value is outside the range. Save that end value and repeat the test around it. Each run covers ±5 % around the current value; if you need more, chain runs.

There is a fine variant, YOLO Perfectionist, from −0.04 to +0.035 in steps of 0.005, for a second run when the first one is already close. You can skip it: a resolution of 0.005 is finer than almost any profile needs.

Orca still offers the old two-pass method. The first pass prints nine blocks with a multiplicative modifier: new = current × (100 + modifier) / 100, so 0.98 with +5 gives 1.029. The second prints ten blocks from −9 to 0 around that result: 1.029 × 0.94 ≈ 0.967. You read it the same way, but it uses more plastic and more time. Use YOLO.

The flow test in Bambu Studio

You launch it from the Calibration › Flow rate tab. Manual mode has two stages, coarse and fine: the same idea as Orca's two passes (Orca is derived from Bambu Studio). The per-block modifiers can change between versions; check them in your version's dialog before doing the math.

Automatic mode exists only on the X1 series, whose Micro Lidar scans the pattern, and needs Bambu Studio 1.7 or later. Bambu excludes transparent, translucent, silk and particle-filled filaments from it, because the lidar cannot read their surface. The A1, P1 and H2D have no lidar: on them you calibrate flow by hand. On any other machine, check its spec sheet for a sensor that can read the pattern before assuming it calibrates flow by itself.

Even on an X1, automatic flow calibration does not run before every print the way Flow Dynamics does. It is a test you run once per filament, and the result is stored in that filament's profile.

Flow in PrusaSlicer and Cura

As of late 2026, PrusaSlicer has no built-in flow test. Prusa's profiles for its own machines and filaments use an "Extrusion multiplier" of 1 for PLA, PETG and ABS, with a 0.45 mm line width on a 0.4 mm nozzle, and Prusa treats this as an advanced calibration, unnecessary on a factory-fresh printer with its own filaments. If you need it (another brand of filament, another nozzle), its knowledge base suggests printing a 40 mm cube in vase mode, with a single wall, and measuring the wall at several points around mid-height: new = current × 0.45 / average thickness. Then you fine-tune by 1–2 % by looking at and feeling the top surface: if plastic piles up next to the walls ("perimeters" in PrusaSlicer), lower it; if gaps open between lines, raise it. Average many readings and let the top surface decide: callipers have the precision limit explained above.

Prusa warns that firmware flow (M221) and the PrusaSlicer multiplier are independent and multiply each other: two settings on the same thing that cannot see each other. And bear in mind that the multiplier does not make up for a worn nozzle (Nozzle and hotend care).

Another option, with a Prusa or any printer Orca supports: Orca has profiles for most printers, Prusa's included. You can run the YOLO test there and copy the value into your PrusaSlicer filament profile (Orca, Bambu Studio, PrusaSlicer and Cura).

Cura calls the field "Flow" (100 % by default) and stores it in the print settings, per extruder, not in the filament profile. It has no built-in test either. Community plugins add calibration parts, such as Calibration Shapes; check that the one you pick works with your Cura version. You read it the same way: on the top surface.

What value to save, and when to distrust it

A normal correction is a few percent, and two brands of the same material differ by a few points. Save it in your slicer's field, one value per filament and nozzle, and save the profile. A modified, unsaved profile is lost when you switch printers (Printer, filament and process profiles).

Where each number lives
Slicer Flow ratio Maximum flow Built-in test
Orca "Flow ratio" (filament) "Max volumetric speed" (filament) Flow ratio (YOLO, two-pass) and max flow
Bambu Studio "Flow ratio" (filament) "Max volumetric speed" (filament) Flow ratio (manual; automatic on X1) and max flow
PrusaSlicer "Extrusion multiplier" (filament) "Max volumetric speed" (filament and print; the lower non-zero one wins) None
Cura "Flow" (%, print settings, per extruder) Hidden on most printers None (plugins)

If the result falls outside 0.90–1.10, the test is pointing at another cause: a wrong diameter in the profile (2.85 instead of 1.75), a partial clog, wet filament, E-steps miscalibrated after reassembling the extruder, or a profile meant for another nozzle diameter. Fix the cause and repeat; do not save the extreme value. The exception is foaming filaments such as LW-PLA, which are deliberately printed with a much lower multiplier to control how much they expand (Functional specialty filaments).

Do not correct the overall flow ratio with the top-surface one ("Top surface flow ratio" in Orca). That field, 1.0 by default, only affects the last layer, and you touch it after the overall flow is right (Top surfaces).

After saving, print an ordinary part with a top surface and a small hole. If the first layer now comes out squashed or starved and it did not before, the Z offset was compensating for a badly set flow ratio: adjust it again (The first layer and bed adhesion).

The max flow test

Every combination of hotend, nozzle, filament and temperature has a melting ceiling in mm³/s. Above it, the core of the filament does not fully melt and the bead comes out thin and cold (Volumetric flow sets the speed, Hotends and how much they can melt). The test finds that ceiling for your combination.

You do not need to repeat it with every spool, only with a new brand or product line, a hardened or high-flow nozzle, another nozzle diameter, another hotend or a big change in temperature. Run it before buying a high-flow hotend too: if your profile's maximum sits below what the test gives, raising it costs nothing. Always start from the value your slicer's profile ships for your printer, which is tested and conservative; the test is for third-party filament, modified hardware or a fast profile.

In Orca it is under Calibration › Max flowrate, and Bambu Studio has the same test. It prints a single-bead wall in which the requested flow rises with height. You set the start, end and step; Orca's defaults are 5 to 20 mm³/s in steps of 0.5. On a fast machine with a high-flow hotend, start higher, for example 15 to 40, so the failure falls inside the range. If the whole part comes out clean, repeat with higher values.

To read it, find the height where the wall changes: gloss turns matt, the wall thins, gaps or a rough band appear, or the extruder clicks. Measure the height right below the first defect with callipers. Maximum = start + height × step, where the step is how much the flow rises per millimeter of height. In Orca's example, 5 + 19 × 0.5 = 14.5 mm³/s. You can also color the preview by volumetric flow and read the value at that layer.

Max flow test piece in gray PLA: glossy at the bottom and, above a certain height, matt, thinner and with gaps
Max flow test piece in gray PLA: glossy at the bottom and, above a certain height, matt, thinner and with gaps
0557.510101512.520152517.53020Height (mm)Requested flow (mm³/s)save here (≈11.6–13.1)failure: 14.5 mm³/smeasure right below the first defectglossy, full wallmatt and thinnergapsmaximum = start + height × step5 + 19 × 0.5 = 14.5
The height of the first defect marks the flow above which the plastic no longer melts fully. The profile stays 10–20 % below it.

Save a value 10–20 % below the failure: if it fails at 24, set 19–21. The test is the best case: a continuous wall, with no retractions or layer changes to recover from. And near the ceiling the plastic comes out cooler than the set temperature, so layers bond worse well before the surface gives it away (Layer adhesion and anisotropy).

The value only holds at that temperature. If you measure it in the upper half of the filament's range, for a fast profile, it stops being valid when you print cooler. Within the same material, brand and even color change the ceiling, so do not copy the number between spools from different lines.

It goes in the filament profile, under "Max volumetric speed". In PrusaSlicer the same field exists in the filament profile and in the print profile: the lower of the non-zero ones applies, and with both at 0 there is no limit. Since it has no test, start from Prusa's values (Prusament PLA, 15 mm³/s with the standard nozzle and 24 with the 0.4 HF) or print a flow tower from a model repository. Cura hides the field on most printers: the speed you type is not capped, so watching the ceiling is up to you (Orca, Bambu Studio, PrusaSlicer and Cura).

Check the value you are about to save, already reduced, against the usual flows for your machine class, listed in Volumetric flow sets the speed. The test's failure point legitimately lands above those figures, which are conservative. But if it lands above one and a half times the top of your class's range with a standard hotend, check the height and the step before you believe it.

When it fails

Typical failures in both tests
Symptom Cause Fix
Every flow block comes out equally rough or ridged The test exceeds the hotend's maximum flow, or has too few top layers Let the test use its own settings and check that the max flow is not capping the top-surface speed
The best block is at one end of the range The real value is outside the test's range Save the end value and repeat around it
The result falls outside 0.90–1.10 Profile diameter, partial clog, wet filament, E-steps Fix the cause and repeat; do not save the extreme
The same spool gives a different flow ratio each time Wet filament or temperature not fixed Dry it and fix the temperature with the tower
The calibrated value changes nothing A firmware or on-screen flow multiplies it, a process-profile setting overrides it, or the profile was not saved or not selected Keep flow in one place only and check which filament profile the plate has assigned
The max flow wall does not fail before the top Range too low Repeat with a higher start and end
The wall fails very low (< ~8 mm³/s in PLA) or erratically Partial clog, heat creep, slipping extruder or wet filament; it is not a ceiling Diagnose the extruder (Extrusion problems) and repeat
A hardened steel nozzle gives less than brass in the same hotend Normal: steel conducts heat worse Allow 5–10 °C more or 10–20 % less flow (Nozzles: size and material)

See also

Design it in KapyCAD

Design parts sized for your printer and your nozzle.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?