kapy academy

Support materials

15 min readUpdated Nov 2026

A bracket whose underside must come out as clean as its top, an internal channel no pliers can reach, an ABS housing with a deep overhang. With a single material, the support sits one layer (about 0.2 mm) away from the part and leaves a rough scar. At the contact layer, a support material either does not stick to the part or disappears afterwards, so the underside prints on top of it with no gap and comes out almost as smooth as a top face. A filament switcher loading dry PVA or BVOH is enough, with no second extruder.

Two ways to close the gap: do not stick, or dissolve

With a single material, the roof of the support and the underside of the part are the same polymer, and they fuse like any two layers (Layer adhesion and anisotropy explains why). To let the support come away, the slicer leaves an air gap of roughly one layer, the top Z distance. The underside is then printed onto beads that sag with nothing beneath them, which is why it comes out rough.

There are two ways round it:

  • Do not stick. Two polymers whose chains do not mix touch without fusing. Functional multi-material parts explains the mechanism; there it is a problem, here it is the whole point. The underside is printed in contact, comes out flat, and the support still peels off.
  • Dissolve. The support is a polymer that dissolves in a liquid that leaves the part alone: water for PVA and BVOH, D-limonene for HIPS. It can stay stuck to the part and it does not matter: it vanishes in the bath. It is the only option for support you cannot reach: internal channels, captive parts, undercuts inside a cavity.
gap ≈ one layerrough facesame materialzero gappeels offnon-bonding pairzero gapdissolvesopen to the outsidesoluble
The same overhang supported three ways. With the part's own material you need a gap and the underside sags; with a non-bonding pair or a soluble support the gap is zero and the face comes out flat. Only the soluble one reaches an internal channel, and only if the channel has a way out.

In the slicer, it all comes down to one setting. With a dedicated support filament at the interface, the top Z distance can be 0; with the part's own material, leave about 0.2 mm or the support will be very hard to remove. In PrusaSlicer the setting is "Top contact Z distance" with the value "0 (soluble)", which also stops the first layer over the support from being printed as a bridge. Support settings covers the rest.

The solubles: PVA, BVOH and HIPS

PVA (polyvinyl alcohol). It dissolves in water and prints cool: nozzle 190–240 °C, bed 35–65 °C. That makes it a partner for materials that also print cool, PLA above all. With PETG it works, but awkwardly, because the temperature gap between the two encourages stringing; for PETG, BVOH is the better choice. With ABS, PC or PA it does not work: PVA degrades at their 240–290 °C nozzle temperatures and softens on their 90–120 °C beds and in their heated chambers. It darkens, chars and clogs the nozzle.

BVOH (butenediol vinyl alcohol copolymer). It belongs to the same family as PVA but tolerates hotter partners. It prints at 190–240 °C with the bed at 50–65 °C. Manufacturers say it dissolves about twice as fast as PVA and works with PETG, ABS, PA and PAHT-CF. Those are marketing claims, not measurements: test the pair before you trust it with a long print.

HIPS (high-impact polystyrene). It dissolves in D-limonene and prints hot, 230–250 °C with the bed at 90–110 °C; that is why it was the classic ABS support for years. Prusa documents the catch: limonene partly dissolves ABS and ASA and can undo the bond between their layers, so Prusa advises against it as a support for those two and recommends it mainly under PETG. If you put it under ABS anyway, use it as a breakaway support: no solvent at all, or a 10–20 s bath to loosen it and the rest by hand. Dissolving all the HIPS off a part takes 12 to 24 hours, according to limonene sellers; treat that as a rough guide.

PVA and BVOH need none of this: water is enough. Warm water speeds up dissolution, but with a PLA part do not go above about 50 °C. The HDT of PLA is 57 °C at 0.45 MPa; in hot water and with no load, a thin part starts to soften below that figure, and it would warp before the support had finished dissolving. BVOH makers say hot water speeds it up a lot, but that only helps with parts that can take it. Allow anything from a few hours to twelve. The support does not vanish all at once: first it swells into a soft gel that you can pull off by hand. Support removal and cleanup has the full routine: changing the water, stirring it, removing the soft mass early, drying the part.

There is no single rule for disposing of the used water. The usual advice is to dilute it heavily and not pour large, concentrated volumes away in one go; check the manufacturer's datasheet and your local regulations.

A mistake many guides repeat: soluble support does not let you design a fully closed cavity. The solvent has to reach the support and the dissolved support has to get out. A sealed cavity keeps its support forever. Leave at least one opening, better two so the water can circulate; as a guide, 3–5 mm in diameter is enough for a small cavity, and the longer and narrower it is, the longer it will take.

Breakaway supports and the PETG–PLA pair

Breakaway supports are filaments formulated to stick poorly to one particular family. At the end of 2026 Bambu, for example, sells three: "Support for PLA/PETG", only for the interface under PLA or PETG; "Support for ABS"; and "Support for PA/PET" (formerly "Support G"), for PA-CF, PA-GF, PAHT-CF and PET-CF, which the maker advises against using with PLA. Polymaker and others sell equivalents. Use the one for your part's family: one from another family either fuses to it or clogs the nozzle.

Two of the maker's instructions apply to any breakaway support:

  • Moisture changes the bond. For Support for PA/PET, Bambu asks you to remove it within two hours of printing and to dry the part if it starts to stick. The support absorbs moisture from the air, softens and grips harder, or leaves residue behind.
  • Contamination weakens the part. For Support for ABS, Bambu asks for at least 800 mm³ (about 0.8 g) of purge when switching from the support to ABS whenever layer strength matters. A foreign polymer inside the part's bead is a weak spot, for the same reason the pair does not stick: it does not fuse.

The option that costs nothing: PETG as the interface under PLA, and PLA under PETG. They do not stick to each other, and both Prusa and Bambu document the combination in both directions. You print it with a zero gap and only the 2–3 interface layers in the second material. On the forums, PETG under PLA is described as reliable and PLA under PETG as less so: pick the first, and test the second before you rely on it.

Which support goes with which filament

The table sums up practical experience, not lab tests: brands vary, and for branded breakaway supports the maker's own table has the final word.

Support material by part material
Part PVA BVOH HIPS Breakaway for its family PETG/PLA pair
PLA yes yes no yes yes (PETG underneath)
PETG / PCTG test it yes yes yes test it (PLA underneath)
ABS / ASA no test it test it, breakaway only yes no
PC no test it test it test it no
PA, PA-CF, PAHT-CF no test it no yes no
PET-CF no test it no yes no
TPU test it no data no data no data no data
PVABVOHHIPSbreakawayPETG/PLAPLAPETG / PCTGABS / ASAPCPA / PA-CF / PAHT-CFPET-CFTPUworks welltest itno / no datapractical guide, test your brands
The same table at a glance: PLA takes almost any support; the high-temperature materials are left with BVOH (to be tested) and the breakaway support for their family, and PVA only goes with the materials that print cool.

The rule behind it lets you judge a pair that is not in the table. The support has to survive the part's bed and chamber. The nozzle temperature only has to match if the nozzle is shared, as on a filament switcher; with dual nozzles or a toolchanger, each material prints at its own. In an enclosed printer, open the door for PLA, PVA or TPU once the bed is above about 45 °C, to prevent heat creep (Enclosures and heated chambers). ABS and PC want the chamber closed and hot, and PVA softens in there. That is why PVA never goes with ABS, and why BVOH, which tolerates more heat, is the soluble that manufacturers pair with ABS and PA.

diagram
Before you buy PVA: if you can reach the support and the underside will not be seen, the part's own material is enough; if it will be seen and the part is PLA or PETG, the other spool is enough.

Interface only: the cheap way to use an expensive support

Slicers let you print only the interface in the support material. PrusaSlicer has the "Soluble interface" and "Soluble full" profiles, and Prusa recommends the interface one when the support stands on the bed. In OrcaSlicer and Bambu Studio you pick the "Support/raft base" filament and the "Support/raft interface" filament separately. Make that your default: the body of the support in the part's material, and only the 2–3 interface layers in the support material.

The reason is purge. Every layer that carries both materials costs one or two filament changes, and on a single-nozzle switcher each change throws away about 0.2–0.8 g of purge (Purge and multicolor waste). A rough estimate with 0.54 g per change, the figure from a Bambu example in PLA: if 120 layers of the part carry support and all of it is soluble, that comes to about 240 changes and about 130 g of purge. If the faces resting on support sit at six different heights and each interface takes 3 layers, printing only the interface in soluble brings that down to 36 changes and about 20 g. Those are minimums: going back from the support to the part usually needs more purge, so the real difference is larger. Fewer changes also cut hours off the print. A toolchanger or a dual-nozzle machine purges far less (Toolchangers, IDEX and dual nozzles); how each single-nozzle switcher works is in Filament switchers: AMS, MMU, CFS and ACE.

There are two cases where it pays to print the whole support in soluble:

  • Support inside a channel or cavity you cannot reach: all of it has to dissolve.
  • Support that stands on the part itself, where a trunk of the part's material would scar a visible face.

The typical failure of an interface-only setup: the soluble interface does not grip the support beneath it, which is in the part's material, and it slides or falls off mid-print. Raise the top interface layers to 3–4 and tighten the interface spacing, so it has more surface to rest on. With tree supports, Bambu advises against using its breakaway filament for the base: keep it for the interface only.

Purge the support material into the support, not into the part: "Flush into objects' support" in OrcaSlicer and Bambu Studio (it needs a prime tower) or the equivalent options in PrusaSlicer.

Keeping them dry

A polymer that dissolves in water also absorbs it from the air, and quickly: the solubles are highly hygroscopic. Wet PVA strings, pops with bubbles, swells, softens and jams in tubes and feeders.

Drying support materials (oven or forced-air dryer)
Material Drying Does it need drying?
PVA 75–85 °C × 8–12 h mandatory
BVOH 60–80 °C × 8–12 h mandatory
HIPS 60–65 °C × 4–6 h recommended
Support for PA/PET (Bambu) 80 °C × 8–12 h per its datasheet
Support for ABS (Bambu) optional helps little, per the maker

Built-in dryers have a temperature ceiling. The AMS 2 Pro reaches 65 °C: it keeps PVA dry if it already is, but it will not rescue a wet spool, and Bambu advises against loading wet PVA or BVOH into it. The AMS HT reaches 85 °C and does rescue it. Store spools in a sealed box or bag with fresh desiccant, below 20 % relative humidity, and on long prints feed them straight from a dry box. If you use calcium chloride, never put it inside anything with electronics: as it saturates it dissolves and drips. Drying and storing filament has the full method.

The opposite extreme fails too: very dry or cold PVA turns brittle and can snap in the tube or the switcher. Avoid tight bends in the tubing.

PVA left sitting hot in the nozzle degrades and chars. On a dual-nozzle machine or a toolchanger, keep the support nozzle's standby temperature low; on a filament switcher, do not leave PVA loaded in the hot nozzle between uses.

When it fails

Symptom, cause and fix
Symptom Cause Fix
The interface is welded to the part wrong pair, or the part's material at zero gap use the support made for that family, or go back to a 0.2 mm gap
The soluble interface slides off the base support it does not grip a base in the part's material more top interface layers (3–4) and denser spacing
PVA strings and blobs on the part PVA wet or too hot dry it and drop the nozzle temperature by 10 °C
PVA jammed in the tube or feeder it has swollen with moisture dry it and do not leave it out in the open
PVA snaps in the tube over-dried or brittle print from the dry box, with no tight bends in the tube
ABS part delaminated after limonene limonene has partly dissolved the ABS or ASA use HIPS as breakaway only or with a bath of a few seconds, or switch to a breakaway support for ABS
Streaks of support color in the walls too little purge from support to part increase the purge volume (800 mm³ or more for Support for ABS)
Switcher jams or errors with PVA wet or over-dried filament, or tight bends dry it and check the path (Multi-material failures)

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?