kapy academy

Washing and curing resin parts

16 min readUpdated Nov 2026

The build plate rises out of the vat with the part hanging from it, glossy and dripping: it is a green part, coated in liquid resin, with its polymer network only partly formed. Washing removes the liquid and curing completes the network, and each step can fail either way. Wash too little and a tacky or white film is left; wash too much and the part swells and cracks. Cure too little and it stays soft, short of its datasheet; cure too much and it turns brittle and yellow.

Everything wet in this process is uncured resin or solvent loaded with it. Liquid resin is never touched without nitrile gloves (and safety glasses), the alcohol is flammable and nothing goes down the drain (Handling resin safely).

diagram
The full routine: the wash loop repeats until the part is dry and matt, and the part's shape decides when the supports come off.

Drain first, then wash in two baths

Leave the plate draining over the vat for a few minutes, tilted so the liquid runs off one corner. Resin that drips back into the vat is neither wasted nor fouling your wash. Pop the part off with the scraper over a paper towel or tray, or wash it still on the plate if your station's basket takes it. Formlabs recommends washing Elastic 50A that way.

A green part, supports still attached, submerged in isopropyl alcohol: what comes off is liquid resin that the wash has to remove before curing.
A green part, supports still attached, submerged in isopropyl alcohol: what comes off is liquid resin that the wash has to remove before curing.

You wash in two baths because solvent cleans worse the more resin it carries. Bath 1, the dirty bath, takes off most of the liquid. Bath 2, the clean bath, takes off the last film. When bath 2 gets dirty, it becomes bath 1, the old bath 1 is retired and bath 2 is refilled with fresh solvent. With that rotation the final rinse always happens in clean solvent and you use as little as possible. For several of its engineering resins (Tough 2000, Rigid 10K, Elastic and Flexible V1), Formlabs asks for two 10 min cycles, the second in fresh solvent.

Agitation does the cleaning, not soaking. A wash and cure station stirs the liquid with an impeller or spins the basket. By hand, shake the part in a lidded jar and work the recesses with a soft brush. Do not use an ultrasonic cleaner with alcohol; Handling resin safely explains why.

Times depend on the resin and the manufacturer. In its Form Wash, Formlabs asks for 5 min for its V5 general-purpose resins and 10 min for the V4 resins and Tough 1500 V2; some engineering resins take 15–20 min. Desktop brands are less precise: for Fast, Siraya Tech gives no minutes and asks you to brush the part until it is clean. As a starting point, use the shortest time that leaves the part clean, a few minutes per bath; if the manufacturer gives a different figure, theirs wins.

Washing too long also ruins the part. Isopropyl alcohol does more than dissolve liquid resin: it soaks into the green network and swells it. The swelling leaves a soft, rubbery skin; as the alcohol evaporates the surface shrinks, is left in tension and crazes or cracks. Formlabs sets limits: a maximum total solvent time of 6 min for High Temp and 20 min for Durable; Elastic 50A can be damaged after 20 min. Flexible and tough resins swell the most. Never leave a part in alcohol overnight.

Alcohol: what strength and when to change it

Use isopropyl alcohol (IPA) at 90 % or more, preferably 99 %. Water does not dissolve conventional acrylate resins, and diluted alcohol, such as the 70 % sold as a disinfectant, leaves a resin film that turns white and blotchy when cured. Formlabs requires 99 % for its biocompatible resins. Some manufacturers accept 95 % ethanol: Siraya Tech recommends it for its Fast. There are also dedicated resin cleaners such as TPM (tripropylene glycol methyl ether), each with its own instructions. TPM barely evaporates: rinse it off with water and dry the part before curing, or it leaves the same residue as alcohol that has not dried.

Alcohol saturates as it loads up with resin. Formlabs recommends changing it once it holds 10 % dissolved resin, and measures that with a hydrometer calibrated in fresh alcohol: resin is denser than alcohol, so density rises as the bath loads up. With some of its resins, parts come out tacky from 5 %. Without a hydrometer there are two signs: the clean bath turns cloudy or takes on color, and parts come out of bath 2 still glossy and slippery.

To stretch the life of the alcohol, leave the dirty bath in the sun in a closed, clear container. The dissolved resin cures and settles at the bottom; decant the clear alcohol and use it as bath 1, never as bath 2, because it still carries components that never polymerize, plus the water the alcohol absorbs from the air. The sludge at the bottom is waste, and a closed container in the sun heats up and builds vapor pressure: Handling resin safely covers how to do this safely.

Water-washable resin is washed the same way, in two baths, but with tap water. Keep washes short (eSUN advises against long soaks) and dry the part completely before curing: even cured, this resin absorbs water, and it cracks if cured wet or over-cured. The rinse water carries uncured resin, so never pour it down the drain.

Dry it before it sees light

The part does not go into the curer until it looks dry and matt. Solvent left on the surface still carries dissolved resin. UV cures that film where it sits and turns it into a white residue, powdery or tacky, that is very hard to remove afterwards. And solvent trapped in pores or cavities expands with the heat of curing and whitens or cracks the part.

Formlabs asks for at least 30 min of air drying after alcohol before post-curing; with some resins about 10 min is enough if you blow the part dry. Use compressed air or a cold-air blower, inside recesses and drain holes too. No heat gun and no hot air on a wet part: alcohol vapor is flammable. If a manufacturer's guide suggests a hair dryer, use it on the cold setting only.

Two identical parts: cured dry (left) and cured still wet with alcohol (right). The light fixes the dissolved resin as a white powder that collects in the corners.
Two identical parts: cured dry (left) and cured still wet with alcohol (right). The light fixes the dissolved resin as a white powder that collects in the corners.

Check before curing: touch the part with a gloved finger. If any areas are slippery or glossy, give it a short dip, one minute, in clean alcohol, or rinse those areas with a wash bottle; then dry it again. Curing does not fix a dirty part.

Hollow parts have to be washed inside as well. Squirt clean alcohol through the drain holes with a syringe or wash bottle, shake the part, empty it, blow air from one hole to the other and leave it to dry for longer, holes facing down. Liquid resin left inside never cures, and trapped solvent cracks the wall days later (where those holes go: Designing for resin).

What curing changes in the part

The printer gives each layer only enough light to solidify and bond to the one before it (How a resin printer works), so the network is left incomplete. Post-curing supplies more 405 nm light so the remaining monomer reacts; heat speeds this up because it gives those loose molecules the mobility to find something to bond to.

Formlabs' 2016 datasheet for Clear, on the Form 2, puts numbers on it, comparing the green part with one post-cured for 60 min at 60 °C under 405 nm light. Tensile strength goes from 38 to 65 MPa; tensile modulus from 1.6 to 2.8 GPa; heat deflection temperature (HDT) at 0.45 MPa from 49.7 to 73.1 °C. Elongation at break drops from 12 to 6.2 %, although on the same sheet notched impact strength rises from 16 to 25 J/m. The part gains strength, stiffness and service temperature, but stretches half as far before it breaks; what each property means for a part is explained in Stiffness, strength and toughness.

Green partPost-cured38 MPa65 MPaTensile strength+71 %1.6 GPa2.8 GPaModulus+75 %49.7 °C73.1 °CHDT at 0.45 MPa+23 °C12 %6.2 %Elongation at break−48 %
Formlabs Clear (2016 datasheet), fresh off the printer and after 60 min at 60 °C under 405 nm light. Curing multiplies strength and stiffness by 1.7; elongation at break halves.

The figures on a datasheet assume the cure it describes. Your part only reaches them with the same light, the same time and the same temperature. For high-temperature resins, thermal post-curing is decisive; see Types of resin.

Post-curing also shrinks the part slightly. Formlabs compensates for it in its print settings; desktop slicer profiles do not always do so. Designing for resin shows how to compensate for it in the model.

How much light, how much heat, how long

What cures the part is the light dose its surface receives (intensity times time) and the temperature, not the minutes on the timer. Power varies a lot from one station to another, so a time from one station or one datasheet does not carry over to another. The 2016 Clear datasheet used 1.25 mW/cm² at 60 °C for 60 min. By default, the second-generation Form Cure cures Grey V5 and Clear V5 in 1 min without heat; for a full cure, 5 min at 60 °C. Newer resins and stronger lamps have cut times by an order of magnitude. Always use the time for your resin and your station.

As of late 2026, desktop wash and cure stations such as Elegoo's Mercury or Anycubic's Wash & Cure combine a turntable with 405 nm LEDs, and almost none of them heat: the LEDs warm the chamber a little, but nothing controls that temperature. The Mercury XS manual gives 2–5 min depending on resin and part size; Siraya Tech asks for 1–2 min for its Fast. Start from the manufacturer's time and adjust it to how the part comes out.

Published cure times: each one holds only for its own resin and station
Resin Station / light Cure
Formlabs Clear (2016 datasheet) 1.25 mW/cm², 405 nm 60 min at 60 °C
Formlabs Grey V5 / Clear V5 Form Cure 2nd gen. 1 min without heat; 5 min at 60 °C for a full cure
Formlabs Tough 1500 Form Cure 2nd gen. 12 min at 70 °C; 12 min without heat to minimize warping
Formlabs Rigid 10K Form Cure 2nd gen. 3 min preheat + 7 min at 80 °C
Formlabs High Temp V2 Form Cure 2nd gen. 15 min at 80 °C, plus an oven post-cure (see Types of resin)
Desktop resins Elegoo Mercury XS 2–5 min depending on resin and size
Siraya Tech Fast Any 395–405 nm station 1–2 min

Formlabs cures most of its engineering resins at 60–80 °C. A hot part cures more fully in less time, but it can distort: thin or long parts sag at 80 °C. That is why Formlabs offers the same schedule without heat for Tough 1500. Most desktop stations do not control temperature. And do not put a part that still holds alcohol in a makeshift oven.

Light only cures what it reaches. The turntable spins so every face turns toward the LEDs; halfway through the cure, flip the part so the face it was resting on gets light. Recesses and the inside of hollowed parts receive less. In dark and heavily pigmented resins, post-cure light only reaches a thin skin; extend the time to cure that skin properly. The core of a thick part was already cured layer by layer by the printer, and what reaches it during post-curing is heat, if your station has any: that is why Formlabs extends the time for bulky parts, which take longer to come up to temperature.

Sunlight works, but you cannot control its dose. It changes with the season, the time of day and the clouds. Window glass blocks the shorter UV but lets through almost all the 405 nm light that cures resin, so behind glass the part cures almost as much and, though more slowly than outdoors, it also degrades. The sun also heats the part and yellows it. Fine for a miniature on the windowsill in summer; not for a part that needs the properties on its datasheet.

If the part is hard but the surface stays tacky, first rule out a dirty bath 2 or a part that went into the curer wet. If it is neither, the cause may be oxygen inhibition: oxygen from the air diffuses into the surface and inhibits the reaction in a thin film. Curing the part submerged in water or glycerine shields the surface from the air. Users report mixed results: try it mostly with flexible and elastic resins; on black resins it can leave a haze.

When to remove supports

Both options work, for different reasons. Before curing, the resin is softer: supports snap or cut cleanly and leave smaller marks. That is the usual approach for miniatures. If you remove them afterwards, they hold thin, long or flat parts in shape while the cure, and the heat if there is any, completes the network and shrinks the part slightly. Formlabs generally recommends removing them after post-curing, and requires it for its biocompatible resins.

As a rule of thumb, cure delicate, thin or flat parts, and anything going into a heated cure, on their supports and cut them afterwards. On small, solid, decorative parts, cut the supports while green, with flush cutters, and cure afterwards. A short second cure after cutting hardens the marks.

Cutting technique and cleaning up the marks have their own article, Support removal and cleanup. Resin is sanded wet, and only once fully cured, as Sanding and smoothing explains.

How to tell it is properly cured

The surface is dry and does not stick to a gloved finger, and there is no liquid sheen left in the recesses. With rigid resins there are two more signs: a fingernail no longer leaves a mark, and a fine test detail snaps with a click instead of bending. On flexible, elastic and tough resins those two tests do not work, because they never get to that point: there the sign is a dry, non-tacky feel plus the datasheet time. Keep curing a flexible resin until it goes hard and you ruin it.

Over-curing exists, but it depends on the resin. Formlabs considers over-curing its resins acceptable unless stated otherwise; yet its own FAQ warns that the part can become more brittle and lose color, and the datasheet of a water-washable desktop resin warns that, over-cured, it turns brittle and cracks. Cure for the time the manufacturer gives, check, and add short rounds only if needed. Clear resins are the first to yellow: cure them no longer than needed and keep them out of the sun.

Daylight and UV keep acting on resin that is already cured, and what they do is degrade it. Next to a sunny window or outdoors, the part grows steadily more brittle and yellow. Unpainted, it is no good outdoors; how to protect it from UV or give a clear part its gloss is in Coatings and epoxy.

When it fails

Symptom, cause and fix
Symptom Cause Fix
Tacky all over Dirty bath 2, short wash or under-curing Brief wash in fresh alcohol, dry and cure again
Hard part with a tacky skin Cured while wet or dirty bath; otherwise oxygen inhibition Dry fully and cure a little longer; try curing under water or glycerine
White, powdery residue, especially in recesses Cured while wet, or saturated or diluted alcohol Before curing: rinse in clean alcohol at 90 % or more, dry and cure. Already cured: wipe with a cloth and clean alcohol; if it will not come off, sand lightly
Cracks or crazing hours or days later Long wash, trapped solvent or resin, over-curing, or water-washable resin cured wet Shorten the wash, dry for longer, add drain holes, cure only for the datasheet time
Soft or rubbery outside when it should be rigid Under-curing: dark resin, shaded faces or a weak station Cure longer, flip the part, check the station's LEDs
Soft inside Under-exposure during printing or trapped liquid resin More curing will not fix it: check exposure, hollow and drain the part
Thin part warped Cured without supports or too hot Cure with supports, with less heat or none
Yellowed part Over-curing or sunlight Shorten the cure, keep it out of the sun; paint or coat it

See also

  • Handling resin safely: gloves, ventilation, the fire risk of alcohol and how to dispose of the dirty bath and rinse water.
  • Types of resin: which families swell most in alcohol, and the thermal post-cure of high-temperature resins.
  • Support removal and cleanup: cutting supports and cleaning up the marks, before or after curing.
  • Designing for resin: walls, clearances, drain holes and post-cure shrinkage.

Design it in KapyCAD

Design parts sized for your printer and your nozzle.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor