kapy academy

Minimum features and text

15 min readUpdated Nov 2026

An FDM printer has two resolutions: in XY it builds with beads about 0.45 mm wide (0.42 in Bambu Studio; the slicer calls each bead a line) from a 0.4 nozzle, and in Z it moves in whole layers, 0.20 mm by default. Every minimum follows from those two numbers (How FDM shapes your design). Each feature has a limit, the smallest thing that prints when everything goes your way, and a design value, the size that always prints, on someone else's printer and in another material. Design to the design value.

Minimums for a 0.4 mm nozzle and 0.20 mm layers
Feature Limit Design value Why
Wall 1 line (≈0.45 mm) 0.9 mm (2 lines); 1.2 mm if handled or loaded A lone bead has nothing to bond to sideways
Free-standing fin ≈0.34 mm (Arachne widens it) 0.9 mm, thicker at the root The nozzle pushes it on every layer
Vertical pin ≈1 mm (one loop, no core) 2 mm if handled; 3 mm if it locates or carries load A tiny layer cannot cool before the next one
Vertical hole ≈1–1.5 mm Undersized pilot, drilled to size It prints small and closes up
Slot in XY 0.4 mm 0.5–0.6 mm The lines bulge and fuse
Gap in Z 1 layer (0.2 mm) 2 layers (0.4 mm), on a layer boundary Height comes in whole layers
Raised text 0.5 mm stroke, 0.4 mm height 0.8–0.9 mm stroke It is a thin wall
Engraved text 0.6 mm stroke, 0.4–0.6 mm depth 0.8 mm stroke It is a slot
Character height 3 mm on a top face, 4 mm on a wall 4 mm on a top face, 5 mm on a wall, in bold On a wall, horizontal strokes come in layers
wallpinslotZ gapraisedengravedlimitdesign1 line 0.45 mm≈1 mm, no core0.3 mm, fuses0.3 mm rounds to 1 layer2 lines 0.9 mm3 mm, with core0.5 mm, open2 layers, 0.4 mmmodel edge
Each feature drawn at its limit (top) and at its design value (bottom), to the same scale. The difference is counted in lines and layers: one line against two, a pin with no core against one with perimeters and infill, a slot that fuses against one that stays open, a 0.3 mm gap that rounds to one layer against one of exactly two.

Walls and fins: count lines, not millimeters

What happens to a wall thinner than two lines depends on the perimeter generator. With variable width (Arachne), the slicer prints any feature larger than about 0.1 mm (its "minimum feature size", 25% of the nozzle in PrusaSlicer and OrcaSlicer). Anything below its "minimum wall width" (85%, about 0.34 mm) gets widened to that value. A fin drawn at 0.25 mm comes out at 0.34, thicker than drawn; one at 0.08 mm disappears. The classic generator drops it or fills it with a fine zigzag. Arachne is the default generator in PrusaSlicer, Cura and OrcaSlicer, and selectable in Bambu Studio. Each is covered in Walls, perimeters and infill.

A line that Arachne prints is still not a wall. A lone bead has nothing beside it to bond to: it wobbles as it is laid down, both its faces are outer surface with the seam on show, and it splits between layers under the first load. Two lines fuse to each other along their full height.

Hence the design values: two lines (0.9 mm) for the wall to exist at all; three lines, 1.2 mm or more, for anything that gets handled, snapped, screwed or loaded. With Arachne, the old rule of drawing in whole multiples of the line width no longer matters; with classic it still holds, and 0.9 and 1.2 come close: two beads fill about 0.86 mm and three, with their overlap, about 1.26 mm.

On a free-standing fin, height matters too. A thin, tall fin is a cantilever the nozzle shoves sideways on every layer: it vibrates, goes wavy and the tip comes out stringy. Thicken the root or taper it (thick at the bed, thin at the top), tie it to the next fin with a rib, or cap it with a small lip.

Before you thicken anything, check how the feature is oriented. A horizontal floor or ceiling 0.6 mm thick is three 0.2 layers and prints fine. The line rule applies to walls built line by line in XY.

A box shelled to 0.6 mm comes out as a single wavy line with holes along the seam. Go to 0.9 mm, and to 1.2 if people will touch it.

Pins, posts and small holes

The trouble with a vertical pin starts at the layers where it stands alone, for example where it sticks up above a lid. That layer is tiny: it prints in a fraction of a second and the nozzle comes back before the plastic underneath has solidified. Minimum layer time slows the head down to give it time to cool, but not below the minimum print speed, and the hot nozzle sitting over the tip keeps it soft. When that is not enough, the tip sags, leans or turns into a blob.

Geometry matters too. Up to 1 mm in diameter, the pin is a single perimeter loop whose sides touch. At around 1.8 mm two perimeters fit with no core, and at 3 mm, two perimeters with infill inside. That is why the design values are 2 mm or more for anything handled and 3 mm or more for a locating or load-bearing pin.

If a pin really has to be small, print two or more copies on the plate so each layer lasts longer and has time to cool between passes, or put a sacrificial tower beside it. Give it a 0.5 mm × 45° chamfer where it meets the plate (The face on the bed) and a fillet where it joins the part. Cooling is set up in Speed and cooling.

Under any side load, a vertical pin snaps along a layer line (Layer adhesion and anisotropy). If it will flex, lay it down, or use a metal pin in a printed hole, as in Splitting large parts.

Small vertical holes print smaller than drawn and, below 1–1.5 mm, tend to close up under the combined effect of the mesh facets, the bead bulging inwards and stringing. The rest of the explanation is in Why holes print small. For a small, accurate hole, print an undersized pilot and drill or ream it to size. Horizontal holes and the sag of their roof are in Designing out supports.

1.5 mm locating pins on a lid print soft and bent, and snap at the base. Take them to 3 mm with a fillet at the base, or press a 2 mm steel dowel into a printed hole reamed to 2.0 mm. Unreamed, a printed 2 mm hole is undersized and the dowel splits the part.

Slots and gaps: in XY they fuse, in Z they come in layers

The bead is squashed against the layer below and bulges sideways, so its edges are not straight. In a 0.3 mm slot the beads on either side touch and fuse. A slot stays open from about 0.4 mm up; a grille, a cut or a letter counter that has to read cleanly should be drawn at 0.5–0.6 mm.

A gap that stays open is not one a part will slide through. Two printed parts that have to move need the clearance in Real printed clearances and, if they print together, the one in Print-in-place clearances.

A horizontal gap measures a whole number of layers. One drawn at 0.3 mm with 0.20 layers comes out at 0.2 or 0.4 depending on where the slicing plane falls. The layer above always prints over air, like a bridge, and sags 0.1–0.2 mm. With a one-layer gap, that sag closes it; with two, air remains. Give it at least two layers (0.4 mm), make it a multiple of the layer height, and put its lower face on a layer boundary, allowing for the first layer if its height is different. Otherwise the gap gets rounded anyway.

In grilles, fewer, wider slots give the same open area and stay open. Leave at least two line widths of air per slot.

A 0.3 mm cut in a grille or in a hinge relief closes up into a solid plate. Open it to 0.5 mm or more, or use fewer slots.

Text: stroke, height and depth

Three numbers decide whether text reads: the stroke width (in XY, counted in lines), the relief height or engraving depth (in Z, counted in layers) and the character height. The limits: raised, a 0.5 mm stroke and 0.4 mm of height (two layers); engraved, a 0.6 mm stroke and 0.4–0.6 mm of depth; characters 4 mm tall on a wall and 3 mm on a top face.

A 0.5 mm raised stroke is a single Arachne line: it reads, but it is fragile and soft-edged. Design raised strokes at 0.8–0.9 mm (two lines) when the text has to come out crisp or survive handling. In an engraving, the groove ends up narrower than drawn because the walls on both sides bulge inwards: 0.6 mm is the minimum and 0.8 mm reads cleanly.

In a regular sans-serif font, the stroke is roughly a tenth of the font size. A character 4 mm tall needs a size of about 5.7 mm (in Roboto the capitals are about 0.7 times the size), and its regular stroke is around 0.57 mm: right at the limit. Use bold or a single-weight lettering font, or go up in size. Avoid serifs and hairline strokes, which vanish, and tight spacing: the gaps between letters and the counters of a, e and o are slots, and below 0.4–0.5 mm they fill in.

Font size is not character height. CAD programs and slicers measure a letter by its body. If you need a particular height, measure the capitals.

In KapyCAD, the sketch "Text" tool (T) sets the font size in millimeters of body: 10 mm of Roboto gives capitals about 7 mm tall. Each letter is a region you extrude for raised text or cut for engraving, and the content and size can be tied to parameters. For SVG artwork with strokes that are too thin, "Offset artwork" pushes the outline outwards and turns a 0.2 mm stroke into a printable one. It is covered in Text, Artwork and Gears.

Which face the text goes on

top facewallbed facelines (XY)layers (Z)lines (XY)layers (Z)2 or 3 layersshort overhangrelief ≤ 1 mmmirrored seen from aboveplateelephant's foot narrows it
The same letter on three faces. On top, every stroke is made of lines and the relief is whole layers. On the wall, vertical strokes are made of lines and horizontal ones of layers, so one comes out two layers thick and the next three; the underside of each horizontal stroke is a short overhang. On the bed face, the engraved groove narrows with the squash of the first layer.

Top face. Strokes are made of lines in XY and the relief is whole layers: this is the best place for raised text. An engraving on a top face has a floor that prints as a top layer; give it at least two layers of depth. Ironing or a monotonic top pattern sharpens it (Top surfaces).

Vertical wall. Here the two resolutions are split stroke by stroke. Vertical strokes are made of lines (XY resolution); horizontal ones of layers (Z resolution). A 0.5 mm horizontal stroke comes out two or three layers thick and the letters look uneven: that is why characters on a wall need 4 mm. On raised text, the underside of each horizontal stroke is a short overhang; with a relief of 0.4 to 1 mm it is a ledge that prints, not a ceiling (Designing out supports). On engraved text, the roof of each groove is a tiny bridge that prints well with strokes of around 1 mm. On top of that, each raised letter is an island: one seam and one retraction per layer, and with them strings and zits between letters.

Bed face. Engraved only: a raised letter would point at the plate and need support. The text has to read when you look at that face from outside; seen from above in the model it appears mirrored, but if you sketch on the bottom face itself there is nothing to flip. The squashed first layer and elephant's foot narrow the groove more than on any other face: give it strokes of 0.8 mm or more and accept softer edges. The text also picks up the texture of the plate (The face on the bed).

Color instead of relief. Text inlaid flush in a second filament on a top or bottom face is the most legible option of all and costs few changes; on a wall it costs one change per layer. The numbers are worked out in Designing for multicolor. Without a filament changer, a single change at the layer where the top relief starts gives two-color text (Four ways to print in color).

Text in the slicer. At the end of 2026, PrusaSlicer (since 2.6), Bambu Studio and OrcaSlicer add text as a part, a negative volume or a modifier, and wrap it onto curved surfaces. That works for a serial number or a label on a downloaded mesh. If the text belongs to the part and must change with its parameters, model it in CAD.

Other nozzles and your own limits

Minimums depend on line width, not on the skill of whoever is printing. With a 0.6 nozzle (0.65 mm line), two lines are about 1.3 mm and raised strokes also need about 1.3 mm. With a 0.2 (0.22 mm line, 0.10 layer), strokes of 0.3–0.45 mm and characters of about 2 mm become printable, at the cost of roughly four times the time for the same volume, and often more, because a 0.2 nozzle takes far less flow. The 0.2 nozzle exists precisely for fine text and miniatures (Nozzles: size and material).

Your printer's real limits come from a coupon of walls, pins and slots that shrink step by step, printed in the material and with the nozzle you actually use (Test coupons).

When it fails

Symptom, cause and fix
Symptom Cause Fix
Text missing from the preview Stroke below Arachne's minimum feature size (or the minimum width with the classic generator), or relief under one layer Stroke ≥ 0.5 mm (design 0.8), relief ≥ 0.4 mm
Raised letters with blobs, counters filled in One-line strokes, gaps between letters < 0.4 mm Bold, larger size, wider spacing
Engraving unreadable on the bed face Elephant's foot closed the grooves Strokes ≥ 0.8 mm, text on the top face or in color
Text on a wall uneven, horizontal strokes thick or missing Height comes in layers Characters ≥ 4 mm, or text on a top face
Thin wall as a single wavy bead, or thicker than drawn Fewer than two lines; Arachne widened it 0.9 mm minimum, 1.2 if functional
Small pins sagging or leaning The layer where the pin stands alone is too short to cool Thicker pins, several copies, sacrificial tower
Horizontal gap closed A single layer of air, or misaligned with the layers Two layers, lower face on a layer boundary
Grille with closed slots Slot < 0.4 mm ≥ 0.5 mm, fewer slots

See also

Design it in KapyCAD

Draw the part with these clearances and walls, and change any dimension later without redrawing it.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?