15 min readUpdated Nov 2026

You open a new spool of PETG: the label says 230–260 °C and the profile retracts 0.8 mm, starting points chosen for someone else's hotend, speed and dryer. Two prints turn them into your numbers: a tower that steps the temperature down, and two pillars with the retraction rising between them. The rule that separates them: temperature decides how freely the plastic flows (the bond between layers, bridges, overhangs, surface finish and part of the stringing), and retraction removes only the ooze of a travel move. Strings between the pillars speak about retraction only once the temperature is fixed.

Before the first test

Both tests belong to the filament calibration: the tower first, retraction last (What to calibrate, and in what order).

Dry the spool first. Wet filament strings, bubbles and pops at any temperature and any retraction, and the giveaways are a hiss and a rough, fuzzy surface (Drying and storing filament). Never raise the temperature to make up for wet filament: you hide the symptom and pick the wrong number.

Print under real conditions. The same nozzle: a hardened steel one conducts heat worse and needs 5–10 °C more than a brass one (Nozzles: size and material). The same plate, the part-cooling fan the filament profile sets, and the door or lid as they will be for the real print; with ABS, ASA or PC, chamber temperature moves the result. Above all, your profile's speed. A tower printed at 40 mm/s does not describe the same machine as one printed at 200 mm/s, because the faster the plastic passes through, the less the hotend melts it.

Check the hotend's maximum temperature before you choose the hottest block. A hotend with a PTFE liner down to the nozzle runs at 240 °C at most: it suits PLA and TPU, and PETG only at the bottom of its range, 230–240 °C. PTFE starts to degrade at around 250 °C and gives off fumes (Emissions and ventilation). The all-metal hotends that current printers ship with reach 290–300 °C (Prusa MK4S and CORE One, 290 °C; Bambu A1, P1 and X1C, 300 °C), and high-temperature hotends for desktop machines reach 320–350 °C. On a PTFE-lined hotend, a PETG tower starts at 240 °C, never at 260 °C.

Also make sure the temperature holds steady: if it swings by a couple of degrees, the blocks stop being comparable. On a machine with open firmware (Marlin or Klipper), tune the PID first; closed machines come tuned from the factory. No mainstream machine calibrates a filament's temperature or retraction on its own: these two tests are yours to run.

The temperature tower

A temperature tower is a stack of identical blocks, each printed 5 °C cooler than the one below. Every block carries the shapes that respond to viscosity: a short bridge, an overhang, a gap the nozzle crosses in mid-air to show strings, and plain walls to judge finish and bonding. The slicer changes the nozzle temperature at the start of each block.

260 °C255 °C250 °C245 °C240 °C235 °C230 °Ccooler ↑stringssagging bridgedrooping overhanggood bandcleanpick herefast profilegaps between layerscrack between layerstemperature settling: do not read here
A PETG tower from 260 to 230 °C, hottest block at the base. The lower blocks show strings, a sagging bridge and a drooping overhang; the upper ones show gaps between layers and a crack splitting two of them. The good band is in the middle. Do not read the start of each block: the temperature has not settled yet.

The range comes from your filament's label or datasheet, not from a generic table. The table is there to catch a mistake: PLA 190–230 °C, PETG 230–270 °C, ABS 240–280 °C, ASA 240–270 °C, PC 260–290 °C, TPU 200–250 °C. A typical tower has 5 to 9 blocks: PLA from 230 to 190 °C in 9 blocks, for example, or PETG from 260 to 230 °C in 7.

The hottest block goes at the bottom and the tower cools as it rises. The base needs the best bonding to carry the rest, and the coolest blocks, the ones most likely to split, sit at the top, where a break takes nothing else down with it.

How to generate one

As of late 2026, each slicer generates it like this:

  • OrcaSlicer: Calibration › Temperature. You give it the start and end temperatures, and the tower steps down 5 °C per block. "Auto-scale for nozzle" is on by default; the model is designed for a 0.4 mm nozzle and 0.2 mm layers.
  • Bambu Studio has a similar test in its "Calibration" menu.
  • PrusaSlicer has no built-in tower. Download a tower model (Printables has plenty) and add a temperature change at each block with "Add custom G-code" on the preview's layer slider, or with a conditional line in "Before layer change G-code". "Add custom G-code" does not work with sequential printing.
  • Cura: the Calibration Shapes plugin from the Marketplace, or a post-processing script that changes the temperature by height.
  • Klipper: TUNING_TOWER on SET_HEATER_TEMPERATURE, with a negative step and the model's block height. For example, TUNING_TOWER COMMAND="SET_HEATER_TEMPERATURE HEATER=extruder" PARAMETER=TARGET START=260 STEP_DELTA=-5 STEP_HEIGHT=10 for 10 mm blocks.

If you write the change yourself, use M104 (set the temperature and carry on), not M109 (wait until it gets there; in Klipper, and with R in Marlin, also when cooling): that wait parks the nozzle on the part and leaves a blob on every block.

The heater lags. When the target drops 5 °C, the nozzle can only cool on its own, and on a small block that can take several layers, which still print at the previous block's temperature. Read the middle and the top of each block, never its first millimeter.

How to read it

Too hot: strings across the gap, a sagging bridge, a drooping overhang edge, a glossy, blobby surface and sometimes a darker shade, a sign the plastic is degrading. Too cold: matt or rough walls, visible gaps between layers, bridge strands that do not fuse to each other, layers you can split with a fingernail, and under-extrusion at the profile's speed. The good band is the run of blocks with a flat bridge, a clean overhang and few strings.

A seven-block PETG temperature tower, 260 °C at the bottom to 230 °C at the top, printed layer by layer on the bed: the two hot blocks (orange) leave strings across the window and to the pillar, sag their bridge and droop their tab; the three middle blocks (blue) come out clean and 245 °C is the pick; the two cold blocks at the top (gray) come out with gaps between layers
The tower prints from the bottom up and the nozzle drops 5 °C each block. At the bottom, too hot: strings, a sagging bridge and a drooping tab. At the top, too cold: gaps between layers. The good band sits in the middle, and one number comes out of it. Layers drawn 1 mm thick; the defects exaggerated so they show.

Bonding is checked by breaking the tower. A block can look perfect and have poorly welded layers. Once you have read the tower by eye, snap it by hand block by block, or bend each one along a layer line with pliers. A block that snaps cleanly along a layer line with little force is too cold for a real part, however good it looks. Layer bonding sets the lower edge of the band (Layer adhesion and anisotropy, Layers splitting apart). For load-bearing parts, stay in the upper part of the good band.

Pick a single number. With a normal profile, the middle of the good band. With a fast profile or a high-flow job, the hotter half of the band, because the plastic spends less time in the melt zone (Volumetric flow sets the speed). For a decorative part, where strings matter more than strength, the cooler half. Save it in the filament profile. The first layer has its own value: the usual choice is to leave it the same or raise it a few degrees.

Each material reads differently:

  • PLA: usually has a wide band. In silk PLA, the sheen changes a lot with temperature: the hotter, the glossier (PLA and its variants).
  • PETG: strings at the top of its range: look for them on the lower blocks, together with bridge sag (PETG, PCTG and other copolyesters).
  • ABS, ASA and PC: print the tower in the closed chamber, as you would the part. Otherwise the cool blocks crack from drafts, not from temperature (ABS and ASA).
  • TPU: the tower works the same way. Read mainly the strings, because retraction does little on soft TPU: the filament compresses instead of pulling back (TPU and flexible filaments).

The tower has a limit: a small block cools quickly and its layers are short, so the fan and the minimum layer time affect it (Speed and cooling). Its surface can come out better than a large part's at the same temperature. Treat the result as ±5 °C and confirm it on a real part.

The retraction test

Retraction comes last among the extrusion tests, with the temperature chosen and pressure advance calibrated. Pressure advance already relieves the nozzle before every stop, and a lower temperature has already removed some of the strings. Orca's own guide says the defaults usually work and that retraction is calibrated after flow and pressure advance. Why the nozzle oozes, and the travel, wipe and Z-hop settings, are covered in Stringing and blobs; they are not repeated here.

The test is two thin pillars a few centimeters apart. On every layer the nozzle travels from one to the other, and the retraction length goes up one step per section. As retraction grows, the strings between the pillars thin out and disappear. The answer is the shortest length that gives a clean section, not the longest one you tried. Slicer towers vary the length, not the speed.

0.0 mm0.2 mm0.4 mm0.6 mm0.8 mm1.0 mmtravelheat-break clog above ~1.5–2 mm (direct)cleanshortest clean section = your valuestringslength = start + n × stepmeasure the height and look up the length in the preview
Two pillars, a travel move between them on every layer and a retraction that rises one step per section; here in 0.2 mm steps, as in a first coarse pass. The first clean section is your value. Going higher gains nothing, and on direct drive, beyond 1.5–2 mm, the heat break clogs.
Retraction test ranges
Direct drive Bowden
Start / end / step in Orca 0 / 2 / 0.1 mm (defaults) 1 / 6 / 0.2 mm (Orca's suggestion)
Step for fine-tuning by hand 0.1–0.2 mm 0.5 mm in a first coarse pass
Useful range 0.4–1 mm (PLA or ABS that comes out clean: 0.2–0.4 mm) 2–6.5 mm
Factory profiles 0.8 mm (Bambu, Orca generic), 0.7 mm (Prusa MK4S and CORE One) 6.5 mm (Cura default)
Retraction speed 25–45 mm/s 25–45 mm/s
Limit clogs above ~1.5–2 mm set by your tube and extruder

In OrcaSlicer the test is under Calibration › Retraction test, with the values in the table. Bambu Studio has a similar test in its "Calibration" menu. In Cura, the Calibration Shapes plugin includes a retraction tower with its post-processing script. PrusaSlicer has no built-in test, and the temperature tower method does not work here: the slicer computes every retraction itself, and G-code added per layer does not change it. That leaves two options: turn on "Use firmware retraction" and change the length by height with M207 (Marlin) or SET_RETRACTION (Klipper), or print several small two-pillar files, one per value.

To go from height to length, measure the height of the first clean section with callipers and look up its length in the slicer. In Orca, find the Calib_Retraction_tower comment at that height in the G-code preview, not the ; retract lines, which can show a shorter length because Orca does not add "Retract amount before wipe" to them. If you would rather work it out: length = start + (section number × step). Each section is a few millimeters tall; check it in the preview rather than assuming it.

If the tower is clean from the first section, which is common with PLA and ABS at a good temperature, you do not need much retraction: Orca suggests 0.2–0.4 mm is enough. If your profile's value is around there, leave it. Do not raise it "to be safe".

If it never comes out clean, stop going up. Above about 1.5–2 mm on direct drive, you pull molten plastic up into the cold part of the heat break, where it solidifies and clogs it (Extrusion problems). Strings that persist across the whole tower come from wet filament, a temperature that is too high or a nozzle leaking plastic through its thread. Dry the spool, check the nozzle is properly tightened and not leaking, and go back in the order. More retraction tuning will not fix it.

Speed goes in a separate test. Keep the profile's value (Cura 25 mm/s, Bambu 30, Prusa 35–45) and change it only if strings remain once the length is set: one more test at a higher speed, within that range. Too fast, and the extruder gear bites into the filament and grinds it (Extruders: direct drive or Bowden).

Leave the travel settings alone during the series. Wipe, Z-hop and "Avoid crossing walls" change how many strings you see, and the tower forces the nozzle across open air, so the result depends on them. Print it with the ones you actually use.

The value is stored in the filament profile's own settings, which override the printer's ("Setting Overrides" in Orca and Bambu Studio, "Filament Overrides" in PrusaSlicer), so other filaments keep the printer's value (Printer, filament and process profiles). On Klipper with firmware_retraction, SET_RETRACTION and a TUNING_TOWER on RETRACT_LENGTH do the same job. In that case, turn on "Use firmware retraction" in the slicer so it sends G10 and G11.

When to repeat them

The temperature tower: with a new filament brand or type, a different material or nozzle size, a new hotend or high-flow block, or a big change in profile speed. Not with every spool from the same line. A filament with a very different formulation, such as silk PLA, glow-in-the-dark or carbon-fiber-filled, does deserve a quick tower.

The retraction test: with a new filament type, a different extruder, when moving from direct drive to Bowden or back, with a new hotend (the length of the melt zone changes the ooze) or after a big change to temperature or pressure advance. If the values change over time without you touching anything, read When your numbers drift. The two prints add up to about an hour on a modern machine.

When it fails

Symptom → cause → fix
Symptom Cause Fix
Strings with a small blob at each end, all over the part Plastic that flows too freely oozes more than any retraction can pull back Temperature tower first, retraction second
Sagging bridges, drooping overhang edges Low viscosity: the bead cannot hold its own weight until it cools Temperature tower; then the fan (Overhang and bridge settings)
Layers you can split by hand Below the band, layers do not weld Temperature tower (and fan, layer time)
Matt, rough walls with gaps, at speed The hotend cannot melt what the profile asks for More temperature for that flow, or a lower flow limit (Flow ratio and max flow tests)
Strings only between separate islands, clean bridges The temperature is right; what remains is ooze during travel Retraction test and travel settings (Stringing and blobs)
Blobs at corners and line ends Excess pressure when braking Neither test: pressure advance (Pressure advance and clean corners)
A vertical line of blobs It is where each layer starts and ends Neither test: the seam (Where the seam goes)
Popping, hissing, a fuzzy surface Water boiling in the nozzle Dry the spool; no test corrects it
The heat break clogs days after raising retraction Retraction raised to remove strings that came from a nozzle that was too hot Go back to a short retraction and lower the temperature with the tower

See also

Design it in KapyCAD

Design parts sized for your printer and your nozzle.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?