A PLA bracket holds a shelf of books on day one and is visibly bent three months later. A PETG clip cracks at the root on the 800th opening. By the datasheet neither was overloaded, but that strength comes from a single pull lasting a few minutes. Under a load held for weeks, plastic keeps deforming: that is creep. Under a load repeated thousands of times, a crack grows from the worst defect: that is fatigue. Which of the two you face decides both the material and the design.

Two identical gray printed brackets screwed to a wall, each carrying a pine board with a book on it. The left one keeps its arm horizontal and its board level; the right one, after months under the same load, has an arm that droops downward and a board that tilts toward the tip.
Two identical gray printed brackets screwed to a wall, each carrying a pine board with a book on it. The left one keeps its arm horizontal and its board level; the right one, after months under the same load, has an arm that droops downward and a board that tilts toward the tip.

Creep: deformation that keeps going

A thermoplastic is not a crystal lattice of strong bonds. It is a tangle of long chains, held together by weak secondary bonds and entangled with each other. Under constant stress the chains uncoil and slide past one another slowly, so the stiffness you measure depends on how long you wait. Polymers are already viscoelastic at room temperature; steel does not creep noticeably until several hundred degrees.

The creep curve has four stages. Loading gives an instant elastic strain. Then comes primary creep, fast at first and then slower and slower, followed by secondary creep, slow and almost steady. If the stress or temperature is too high, tertiary creep sets in, accelerates and ends in creep rupture. A good design never gets past secondary creep. The part always moves; what matters is how much strain it has built up by the end of its service life.

TimeStrainYour design limitElasticRuptureTertiaryWarmPrimarySecondaryRoom temperatureUnloadPermanent set
The same load at room temperature and when warm. At room temperature the strain levels off and, once unloaded, leaves a permanent set. When warm the curve accelerates, soon passes the limit your design allows and ends in rupture.

When you unload, part of the strain recovers over time and part is permanent. That is why a hook that carried a heavy bag for a month stays slightly open after you take the bag off.

Datasheets for injection-molding plastics give the creep modulus (or apparent modulus): the effective stiffness after a time under load. The datasheet for an injection-grade polycarbonate, Covestro's Makrolon, gives a tensile modulus of 2,400 MPa and, as creep modulus, 2,200 MPa after 1 hour and 1,900 MPa after 1,000 hours, at 23 °C and strains up to 0.5 % (ISO 899-1). Even PC, one of the common plastics with the best creep resistance, deflects about a quarter more after six weeks than the short-term modulus predicts. Use the ratio as a multiplier:

deflection after 1,000 h ≈ initial deflection × E / E_creep

In a printed part the real creep modulus is lower still and the deflection larger, because the voids and the welds between layers add their own strain. And as of late 2026, filament datasheets almost never give a creep modulus: take it from the datasheet of a molding grade of the same polymer (ISO 899-1) as an optimistic bound, or measure it.

A brittle polymer gives no warning. Under sustained tension PLA can craze (whitish microcracks) and break with almost no prior bending, whereas a tough polymer bends a long way before it breaks. The break starts where a sustained strain meets a seam or a notch. That is why a PLA press fit cracks days after assembly.

Heat speeds up creep

Chain mobility rises quickly with temperature and jumps at the glass transition (Tg). Below Tg an amorphous plastic is glassy and creeps slowly. Close to Tg the modulus collapses and creep goes from months to hours. Approximate Tg values: PLA 55–60 °C, PETG ~80 °C, ABS ~105 °C, PC ~145 °C. A semi-crystalline polymer (PA, PP, PEEK) keeps its shape above Tg thanks to its crystals, but creeps far more in that range. PP has its Tg below 0 °C, so it creeps at room temperature. Dry PA has its Tg between 40 and 70 °C, lower still once it has absorbed moisture.

The heat deflection temperature (HDT) comes from a short test under a fixed load. Use it to compare materials and set a margin, but it does not tell you how hot the part can get without creeping. Under load, design 15–20 °C below the HDT at 0.45 MPa if the plastic is amorphous (PLA, PETG, ABS, ASA, PC), and 15–20 °C below the HDT at 1.8 MPa if it is semi-crystalline, with or without fiber (nylon, PP, PA-CF, PET-CF, PPA-CF, PPS-CF). Under a sustained load, PLA is only comfortable below about 30 °C and its limit under load is around 40 °C; PETG's is around 50 °C. The table by material is in Heat, cold, sunlight and chemicals.

In practice, a PLA hanger by a sunny window sags within days at a stress it would carry for years at 20 °C. In summer, a car's dashboard in the sun reaches 70–100 °C. A loaded part there needs a fiber-filled compound: PA-CF, PET-CF or PPA-CF. Unloaded or in the shade, in the console or the glovebox, ASA, PC or annealed PLA-HT will do, and PC wherever it takes knocks. Inside a car, never PLA or PETG. Fiber does not get you round Tg either: a PPS-CF used hot works far above its Tg (~90 °C) and creeps under sustained load even though its HDT is well over 200 °C.

Because of physical aging, a freshly printed part is slightly less dense and creeps more than it will a few weeks later. In semi-crystallines, annealing raises crystallinity and cuts both creep and the loss of stiffness when hot (Annealing and strengthening).

Printing resins creep too. Standard and "tough" resins have low HDTs and become more brittle with time and UV light: do not use them for sustained load unless it is an engineering grade whose datasheet gives the HDT.

Relaxation: when the displacement is fixed

Relaxation is the same phenomenon with a different boundary condition. Under constant load, strain grows: a bracket, a hook, a part standing on a printed foot. Under constant displacement, stress falls: this is stress relaxation. It happens in a screw tightened against plastic, in the boss of a heat-set insert, in a press-fit pin, in a snap-fit arm left deflected, in a plastic clamp, or in a gasket squeezed between two printed flanges.

CreepConstant loadTimeLoadStrainRelaxationConstant displacementTimeTimeDisplacementStress
Creep and relaxation are one phenomenon seen from both sides. With the load fixed, the bracket gives way. With the position fixed, the screw loses preload.

Screws and heat-set inserts lose preload within weeks, and faster when warm. A press fit loses a good share of its initial stress within days. More interference buys little long-term grip, because the extra strain either relaxes away or crazes the plastic, and it does add crack risk. For pins up to 10 mm, stay at 0.05–0.10 mm of diametral interference, measured from the point where your fit coupon gives zero clearance. A snap-fit arm that sits deflected at rest loses its grip.

The cure is mostly mechanical:

  • A wide washer or a flanged head, to lower the bearing pressure.
  • A compression limiter (a metal sleeve), so the clamping force goes through metal and not plastic.
  • Retightening once, after a day or two.
  • Snap fits with the arm straight at rest and the hook sitting against its stop, not forced.
  • A mechanical lock for press fits: a shoulder, a barb, flats or glue.

Watch the chemistry too. Sustained stress plus an aggressive agent crazes PC, ABS and their blends within days: oils, greases, isopropyl alcohol, sun cream. Never put liquid threadlocker on PC or ABS.

The dimensions are in Self-tapping screws in plastic, Designing for heat-set inserts, Captive nuts and clearance holes and Choosing the fit: clearance, transition, interference.

Fatigue: damage that builds cycle by cycle

Each load cycle pushes a crack that started at a stress raiser a little further. When the remaining section can no longer carry the peak load, the part snaps, with almost no bending. That peak stress can sit far below the static strength, which is why a static calculation misses fatigue: it checks a single cycle. The fracture surface gives it away: a smooth zone, sometimes with beach marks, where the crack grew slowly, and a rough zone where the rest let go.

The S-N curve (Wöhler curve) plots stress, or percentage of strength, against the logarithm of the number of cycles. Unlike steel, polymers have no reliable fatigue limit: there is no stress below which they last forever. So you design for a specific number of cycles.

Stratasys published a fatigue study on parts printed on an F900: 0.254 mm layers, ASTM D7791, load ratio R = 0.1 (the minimum load is 10 % of the maximum), 5 Hz and 23 °C at 50 % RH. The test stopped at one million cycles, each percentage is of the ultimate strength in the same orientation, and there were two to four specimens per level. Nylon 12CF (a PA12-CF) printed on edge (XZ) reached one million cycles at 40 % of its strength without failing. At 50 % it lasted on average about 136,000 cycles, at 60 % about 34,000, and at 80 %, 427. A PEKK with nanotubes, Antero 840CN03, also passed a million at 40 %. ULTEM 9085 (a PEI), in the same orientation and at only 16 % of its strength, lasted on average about 376,000 cycles.

Stress (% of strength)Cycles02040608010010²10³10⁴10⁵10⁶1 millionRunoutPA12-CFPEI 9085Stratasys, ASTM D7791, R = 0.1, 5 Hz
Two printed materials fatigue-tested under the same conditions. One passes a million cycles at 40 % of its strength; the other, at 16 %, fails on average before a million.

The fraction of static strength a printed material withstands for a million cycles varies by a factor of 2 to 3 between materials. There is no universal ratio, and nobody has published the S-N curve for the PLA coming off your printer.

In a printed part, the fatigue crack starts in specific places:

  • The valleys between layers, a row of notches perpendicular to the load.
  • The seam, which lines up the defects of every wall start and end in a single vertical.
  • The voids between beads and the joint between walls and infill.
  • Sharp inside corners.

In the Stratasys study, specimens printed upright (ZX) withstood a much lower stress in MPa than those printed on edge, in the same proportion as in static tests. Apply the orientation factor to fatigue too, once. Cyclic tension across the layers is still the worst case, because it starts from a lower strength and its notches lie across the load.

If the load oscillates without ever dropping to zero, the part creeps while it fatigues. Check the deflection under the mean load, as if it were sustained.

Plastics also have a problem steel barely knows: self-heating (hysteretic heating). Each cycle, the polymer dissipates part of the energy as heat. A part that vibrates fast with large strain, such as a fan mount on a motor, warms up, softens and fails sooner. The thicker the section, the worse it gets, because a thick section sheds heat poorly. That is why labs test plastics at a few hertz.

When the cycle imposes a strain (snap fits, living hinges, flexures), compare the cyclic strain with the repeated-use column in Print-friendly snap fits, not the single-assembly one: PLA 1–1.5 %, PETG 2 %, ABS/ASA 1.5 %, PC 2 %, conditioned PA 4 %, PP 6 %. In the folding test cited in Living hinges and flexures (Balderrama-Armendariz et al., 2019), printed PP reached a million cycles and TPU passed two million, while the other materials tested broke before 1,000 cycles.

Which material resists which load

The ratings are qualitative: apart from the data cited, there are no reliable creep or fatigue measurements for printed filament.

Behavior under sustained and cyclic load
Material Sustained load, room temperature Sustained load, warm Repeated load or flexing Why
PLA Comfortable only at low stress and below ~30 °C Its limit under load is around 40 °C Poor: brittle cracks at notches and seams Tg close by, little elongation
Tough PLA (PLA+, Tough+) Worse than plain PLA Poor Somewhat better than PLA Softer, more deformable
PETG / PCTG More initial deflection than PLA (lower modulus); no reliable data on its long-term creep Creeps with some heat Better than PLA Tougher and more flexible
ABS / ASA Fine Better margin (Tg ~105 °C) Moderate Amorphous with high Tg
PC Best without fiber Very good Notch-sensitive Tg ~145 °C; needs generous fillets
Unfilled PA Creeps more than PC Poor, worse when wet Excellent once conditioned Tough, but soft with water and heat
PP Poor: a hook slowly opens Poor Best in flexing Tg below 0 °C, very tough
Fiber-filled (PA-CF/GF, PET-CF, PPA-CF) Best along the bead Best along the bead Good under cyclic load along the bead; poor in clips and flexures The fibers work in XY; in Z the matrix rules
TPU Cannot carry load Cannot either Takes millions of flexes if free of notches Creeps and recovers slowly

Three caveats. In fiber-filled grades the bead carries load along its axis, but between layers the matrix does the work, and datasheets give 25–55 % of the XY strength in Z; for design, assume 30 % (Layer adhesion and anisotropy). Their elongation is also low: do not use them for clips in repeated use. And at room temperature, PLA holds a light sustained load about as well as PETG: no reliable data on printed parts says which creeps more. PETG only wins when the part gets warm. For a sustained load, use PC or ASA, or a fiber-filled filament if the part is not a spring.

Each family has its own article: Polycarbonate and its blends, Nylons and polyamides, Polypropylene and Carbon and glass fiber filaments. For industrial temperatures and loads, PPS, PEEK, PEKK and PEI.

Designing for time

  1. Identify the load. Is it static (seconds), sustained (hours to years) or cyclic? If cyclic, count the cycles. A clip you open twice a day for five years adds up to about 3,650. A part on a motor at 25 Hz does 90,000 cycles an hour. Write the number down before you choose a material.
  2. Size with margin. Use a safety factor of 4 or more for sustained, cyclic or hot loads, or where someone could get hurt, as in Estimating whether a part will hold. A factor of 4 covers moderate cycle counts, in the thousands. If the part racks up hundreds of thousands of cycles or vibrates, not even that guarantees anything: the ULTEM broke at 16 % of its strength. There, test the part, change material, add metal or do not print it. Do not multiply the orientation factor (0.5 or 0.3) by an extra one "because the load crosses the layers": it already includes that.
  3. Under sustained load, size for deflection as well. Work out the deflection with the short-term modulus and multiply it by E / E_creep. With no data, assume at least the PC figure, about 25 % more deflection, and a good deal more for a printed, hot or damp part. Depth and ribs buy stiffness faster than a change of plastic: bending stiffness grows with the cube of the depth (Ribs, gussets and fillets).
  4. Orient, and look after the notches. Run the beads along the tension, sustained or cyclic, so it does not cross the layer lines. Move the seam off the most loaded face (Where the seam goes) and fillet every inside corner the load passes through.
  5. Walls before infill. The crack starts at the surface and at the joint between walls and infill. Near loaded areas, add walls; where stress concentrates, make the part locally solid with a modifier (Modifiers by region and height).
  6. Thermal margin and preload. Apply the 15–20 °C margin below the HDT, and treat every screwed or press-fit joint as a joint that relaxes.

When it fails

Symptom, cause and fix
Symptom Cause Fix
The bracket or mount sags slowly, no crack Creep under sustained load, worse when warm More depth or ribs, PC or a fiber-filled grade, stay below HDT − 15–20 °C
It sagged after a hot day or inside the car It worked near or above its Tg A higher-HDT material: ASA or PC unloaded; under load in a car, PA-CF, PET-CF or PPA-CF
The screw or insert loosens within weeks Stress relaxation in the boss Washer or flanged head, compression limiter, one retightening, insert instead of self-tapper
The snap fit or press fit has lost its grip, no crack Relaxation of a deflected arm or of the interference Arm straight at rest, mechanical lock, no added interference
Clean crack at the root of a clip after many uses Fatigue from a notch or a layer line Fillet the root, beads along the arm, strain within the repeated-use limit, PETG/PA/PP
Flat break along a layer line after vibration Cyclic tension across the layers or at the seam Reorient, move the seam, print hotter or in an enclosed printer for better layer welding
Crazing or a crack next to a screw in PC or ABS Sustained stress plus a chemical agent Remove the threadlocker, grease or solvent; lower the preload

How to test it

For creep, hang a dead weight from a coupon or from the real part and read the deflection with a dial indicator or against a mark on a ruler, at 1 hour, 1 day and 1 week. Plot it against time on a logarithmic scale: creep usually grows almost in a straight line on that scale, so extend the line out to your service life. For fatigue, cycle it by hand or with a cheap servo or motor, and count. If it will run hot in service, run the hot test at the service temperature under load: 40 °C for PLA and 50 °C for PETG. Test coupons and Iterate and measure explain how to set this up.

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?