kapy academy

Metal filaments and sintering

16 min readUpdated Nov 2026

You want a steel knob or a medallion that looks like bronze, and the shop has two spools that say "metal". One gives you a PLA part about three times heavier than in plain PLA, which polishes up to a metallic shine. The other, after a furnace, gives you a part in 316L stainless steel, metal through its whole volume and around a sixth smaller. Metal-filled filament makes a heavy plastic part; bound metal filament makes a preform that only becomes metal once it has been debound and sintered, in your own kiln or at a service.

Two filaments, one label

Metal-filled filament is PLA loaded with metal powder. That covers colorFabb's bronzeFill, copperFill and steelFill, the Proto-pasta range and the "Metal PLA" of many brands. colorFabb states 80 % metal by weight and a filament density of 3.9 g/cm³, against 1.24 g/cm³ for PLA. It prints like PLA, only slower and through a hardened nozzle.

Bound metal filament (or sinterable filament) carries 87–90 % metal powder by weight in a binder designed to be removed later. As of late 2026, three families are well known:

  • Ultrafuse (Forward AM): ~90 % metal by weight in a POM-based binder, inherited from BASF's metal injection molding (MIM) feedstocks. It is debound catalytically.
  • Filamet (The Virtual Foundry): PLA binder, 87–90 % by weight in the copper grade. It is debound by heat in the same kiln that sinters it.
  • Zetamix (Nanoe): debound first in a solvent, then by heat.

The filament is dense and the spools are heavy: Ultrafuse comes on spools of up to 3 kg, and copper Filamet sits around 4.5–4.7 g/cm³.

Percentage by weight is misleading. What counts is volume. With 80 % bronze by weight (about 8.8 g/cm³) in PLA (1.24):

  • metal: 0.8 / 8.8 = 0.091 cm³ per gram of filament
  • PLA: 0.2 / 1.24 = 0.161 cm³
  • metal fraction by volume: 0.091 / (0.091 + 0.161) ≈ 36 %
  • density: 1 / 0.252 ≈ 3.97 g/cm³, the datasheet figure

A third of the volume. Some particles touch, but each one is wrapped in a film of PLA, which insulates: there is no path for a current. And there are too few of them to hold the shape on their own: take the plastic away and you are left with a heap of powder, not a part to sinter. With 90 % steel by weight (about 7.9 g/cm³) in a POM binder (~1.4 g/cm³) you get 0.114 / (0.114 + 0.071) ≈ 61 % metal by volume, and a filament density of about 5.4 g/cm³, the value in the Ultrafuse safety datasheet. That is packed powder, the same proportion as MIM feedstock: when the binder goes, the particles stay in contact, the shape holds and they can sinter.

80 %by weight36 %by volume90 %by weight61 %by volumemetal-filled PLAbound metalparticles insulated by plasticbindercontact
At 80 % by weight, bronze fills a third of the volume and every particle is wrapped in plastic: the part is still plastic. At 90 % by weight, steel fills around 60 % and its particles touch: once the binder is removed, they can bond.

Neither part conducts electricity as it comes off the printer; The Virtual Foundry says so explicitly about Filamet. Conductive filaments are a different thing, covered in Functional specialty filaments.

Metal in PLA: weight, feel and polish

What it gives you is weight: about three times that of PLA for the same volume. That suits counterweights, paperweights or chess pieces that do not tip over. It feels cold, because the metal draws heat from your hand. And the surface sands and polishes. Abrasive paper cuts through the polymer skin and exposes the particles; fine grits then burnish them. The usual sequence is progressive grits, then steel wool, then a metal polish. The dark residue left in the recesses reads as patina. Copper and bronze oxidize, and you can patinate them on purpose. The grit progression is in Sanding and smoothing.

The price: the part is weaker and more brittle than the PLA it is made from. The Virtual Foundry warns that it does not carry load the way its base PLA does. Do not expect reliable strength figures on the datasheets, and do not use it for load-bearing parts. It has the same heat resistance as PLA, because it is PLA (PLA and its variants). And it is abrasive.

Print it as PLA, within the roughly 10 °C window on the datasheet, at moderate speed and with a hardened nozzle. A 0.6 mm nozzle reduces clogs from particle clumps; the detail is in Nozzles: size and material. On the spool the filament is stiffer and more brittle than PLA: avoid tight bends in a Bowden tube and check with the maker before loading it into a filament switcher.

Silk PLAs and those with metallic glitter only look like metal: the flakes reflect light, but there is nothing to polish. They are in Decorative filaments.

Printing bound metal

What comes off the printer is the green part: metal powder held together by binder. The Ultrafuse user guide gives these starting values:

Starting values for Ultrafuse (Forward AM guide)
Parameter Value
Nozzle 0.3–0.8 mm, 245 °C
Bed 90–105 °C, with Dimafix or Magigoo Pro Metal
Speed 25 mm/s
Maximum flow with 0.4 mm 25 cm³/h (about 7 mm³/s)
Layer height 0.10–0.25 mm (≤ 60 % of nozzle diameter)
Walls 1–3
Solid infill 105 %, rectilinear, 20–35 % overlap
Part cooling fan Off (bridges only)
Enclosure Recommended

All that slowness and extra material has a reason: every void in the green part survives as a void or a crack in the metal. Sintering does not close cracks. That is why Forward AM prefers over-extrusion to gaps, and why gap fill between walls matters when they are thin (Walls, perimeters and infill). The fan cools each layer before it fuses to the next, and that weak bond opens up in the furnace as delamination. The enclosure prevents warping.

The nozzle wears faster than with a normal filament. A hardened steel one lasts longer; brass will do if you replace it every 3 kg of filament, according to Forward AM. For Filamet, The Virtual Foundry asks for a hardened nozzle of 0.6 mm or larger.

An Ultrafuse green part is tough enough to drill, sand or machine before the furnace, and it is far cheaper to do it now than in steel. A Filamet green part is fragile. In both cases, let it cool before you lift it off: a warped base becomes a crack in the top face after the furnace.

Any current enclosed printer with a hardened nozzle and a 100 °C bed will do. The spool is heavy: put it on a holder that turns smoothly.

From green to metal: why it shrinks

Debinding (green to brown). The binder goes. Each product does it its own way:

  • Ultrafuse: catalytic debinding in gaseous nitric acid diluted in nitrogen, which advances 1–2 mm per hour from every outer surface. Industrial furnace only.
  • Filamet: thermal, in the kiln itself, with the part buried in refractory ballast and sintering carbon inside a crucible. Copper and bronze have a debinding stage at 482 °C.
  • Zetamix: an acetone bath (24 h at 40 °C for 316L, according to its datasheet), then thermal up to 650 °C in argon-hydrogen.

The brown part is packed powder held together by a remnant of secondary binder. It is very fragile.

Sintering (brown to metal). The part is heated close to its melting point without reaching it. Atoms diffuse to reduce the total surface area, sintering necks grow between neighboring particles, the pores close and the part densifies. Copper Filamet sinters at 1052 °C (copper melts at 1085 °C) and bronze at 885 °C. 316L needs around 1350 °C in a hydrogen atmosphere, which also strips carbon and oxygen from the steel.

The shrinkage is huge because the pore volume disappears. If the metal fills 61 % of the volume and the part densifies fully, linear shrinkage is 1 − 0.61^(1/3) ≈ 15 %. The makers' figures come out somewhat higher, because the green part is not solid: there are gaps between beads that close too.

Linear shrinkage after sintering, per manufacturer
Product XY Z Final relative density
Ultrafuse 316L 16.6 % 19.3 % ≈ 98 % (7.85 g/cm³)
Filamet copper and bronze ~5–7 % — 90–95 %
Filamet stainless steel 10–12 % — 90–95 %
Zetamix 316L 13 ± 1 % (distributor figure) — 90–95 %

Some of The Virtual Foundry's pages give up to 10 % for copper and bronze. Filamet shrinks less because it never fully densifies: it stops at 90–95 % relative density. Some users scale Zetamix to around 118 %, more than the 115 % that 13 % implies: calibrate against your own furnace.

It shrinks more in Z for two reasons. In the furnace, gravity squashes the part while it is soft. And in the stack of layers, the gaps between beads of successive layers close. Forward AM notes that print direction matters more than orientation in the furnace.

binderporesintering neckXY −16.6 %Z −19.3 %printedfinalscale factorXY 120 % · Z 124 %green partbrown partsintered partdebindsinter
Debinding leaves pores where the binder was; sintering closes them with necks between particles and the part shrinks, more in Z than in XY.

The scale factor is 1 / (1 − S), not 1 + S. With 16.6 % shrinkage you scale to 120 %, not 116.6 %; with 19.3 %, to 124 %. Forward AM's example: a 10 mm cube is printed at 12 × 12 × 12.4 mm. Scale each axis separately in the slicer, never with one uniform percentage.

Those figures assume the maker's print profile. An over-extruded or under-extruded green part has a different density and shrinks differently. Print a test coupon of known dimensions, sinter it, measure it and correct the per-axis factors. Even then, expect a few tenths of a millimeter of error and finish critical fits in the metal: tap the threads, ream the holes. Polymer shrinkage is another story, a few tenths of a percent, covered in Shrinkage and dimensional stability.

Designing for the furnace

These rules come from the Ultrafuse guide and make a starting point for any bound metal.

Design rules for bound metal (Forward AM guide)
Rule Value Why
Green size ≤ 100 × 100 × 100 mm; better ≤ 60 mm Furnace ceramic plates; bigger means more risk
Base Flat, no warping The part slides over the plate as it shrinks
Slenderness Height:width < 3:1 Near sintering temperature the part sags
Unsupported wall Height:thickness < 6:1 Beyond that, cracks and collapse
Green wall ≥ 1 mm A single 0.4 mm bead distorts
Infill of hollow parts ≥ 60 %, gyroid, grid or triangles Below 50 % not recommended
Threads Tap-drill hole, tapped afterwards A printed thread does not fit

The flat base is the rule that saves the most parts. As it shrinks, the part drags across its plate; a base that rocks tilts and cracks. Sand the base flat. Services use a shrink plate, a base that shrinks with the part to remove the friction.

Near sintering temperature the brown part sags like hot glass. Overhangs need supports that also go through the furnace. Put fillets or chamfers at changes of section: sharp edges concentrate thermal stress and open cracks between layers. Avoid going abruptly from thick to thin, because debinding takes longer the thicker the section.

The minimum wall applies to the green part, which is scaled up: a 0.9 mm wall in the design comes out at about 1.08 mm green. Design to the final size and check the green size: for bound metal, design walls of at least 0.85 mm, which × 1.2 gives 1 mm green.

Infill saves a lot of material: in the maker's example, 60 % rectilinear cut the mass by more than 40 %. And you can print closed hollow volumes, which laser powder bed fusion cannot do without drain holes.

Who sinters the part

Ultrafuse is not a home process: catalytic debinding uses gaseous nitric acid and sintering uses hydrogen. You print and send the green parts to a debind-and-sinter service. The guide names Elnik and DSH, and Forward AM ran its own. Note: Forward AM, the former BASF division, filed for insolvency in November 2024, and Stratasys bought its assets in May 2025. Before you plan, check which services are still running and on what terms.

Filamet uses only heat, so you can run the whole process at home with a programmable electric kiln (muffle or ceramic) that reaches sintering temperature, refractory ballast in a crucible and carbon to limit oxidation. That is realistic for copper and bronze. Stainless sinters higher than a typical ceramic kiln reaches: it needs a high-temperature furnace or a service. Debinding burns off the PLA binder and gives off smoke: vent it outdoors (Emissions and ventilation). A kiln at 1000 °C calls for its own precautions against fire and burns.

Zetamix splits the work: you can do the acetone bath yourself, and the thermal stage and sintering in argon with 2.5 % hydrogen usually happen at a service. That diluted atmosphere is easier to handle than pure hydrogen, so more furnaces can run it. Nanoe sells sintering vouchers through its distributors.

There are, or were, closed systems that did all of this with their own printer and their own furnace: Markforged's Metal X (Nano Dimension acquired Markforged in April 2025) and Desktop Metal's Studio System. Desktop Metal, also part of Nano Dimension by then, filed for Chapter 11 bankruptcy protection in the US in July 2025.

What metal you get

The datasheet for sintered Ultrafuse 316L (version 2.0) gives:

Sintered Ultrafuse 316L (Forward AM datasheet, v2.0)
Property Flat (XY) Upright (ZX)
Density 7.85 g/cm³ 7.85 g/cm³
Tensile strength 561 MPa 521 MPa
Yield strength Rp0.2 251 MPa 234 MPa
Elongation at break 53 % 36 %

The anisotropy survives the furnace. Parts printed upright are weaker, and the drop in ductility in Z comes from defects at the bonds between layers (Layer adhesion and anisotropy). Compared with the plastic it replaces, the part has about fifteen times the strength of printed PLA (about 35 MPa in XY), is ductile rather than brittle and takes temperatures no polymer survives. It is not the equal of wrought steel or a MIM part: it comes close in strength, but residual porosity shortens its fatigue life.

Filamet copper and bronze, at 90–95 % density, conduct heat and electricity worse than solid copper and are less strong. They suit heat sinks, electrodes, art pieces or jewelry.

Out of the furnace, the steel is matt gray and keeps its layer lines. Treat it like any stainless part: blasting, vibratory finishing, polishing, machining and, for 17-4 PH, heat treatment.

diagram
For looks and weight, metal-filled PLA is enough. A small, chunky metal part can come from bound metal; a thin, large or precise part, or one in aluminum or titanium, goes to another process.

When another process makes more sense

Bound metal makes sense for a few small, chunky parts in 316L, 17-4 PH or copper, if you already own the printer and can wait for the service queue. Debinding and sintering take days, and each iteration is measured in weeks.

Order the part from a laser powder bed fusion (SLM/DMLS) or binder jetting service when you need tight tolerances, thin walls, large parts, aluminum or titanium, or a fixed quote with no trial runs. How each process works is in Five ways to 3D print, and when ordering pays off, in When to order the part instead.

When it fails

Common symptoms with metal
Symptom Cause Fix
Crack in the top face after sintering Distorted or warped base, or part lifted off while hot: the cause is on the bed, days before the furnace Let it cool before removing, sand the base flat
Layers split after sintering Part cooling fan on, or gaps between layers Fan off, more temperature, less speed
Tall part sagged Height:width ≥ 3:1 or unsupported wall ≥ 6:1 Redesign or add supports that go into the furnace
Dimensions off after sintering Uniform scaling, or over- or under-extruded green part Scale per axis with 1 / (1 − S) and calibrate with a measured coupon
The metal-filled PLA part breaks under a light load It is more brittle than the PLA it is made from Use it for weight and looks, never for load
Clogs with metal-filled PLA Particle clumps in a 0.4 mm nozzle 0.6 mm hardened nozzle

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?