A figure that looks carved, a vase, a sign that glows at night or a lampshade is judged on its finish and carries almost no load. Nearly all decorative filaments are PLA (sometimes PETG) with something added that is not plastic: wood flour, mineral particles, metal or mica flakes, glass microspheres, glow powder, or a second color bonded to the first. That filler decides which nozzle you can use, how the filament prints and what the part looks like. It almost always costs strength between layers, so any structure goes in another material.

What the filler does: nozzle, flow and strength

Fillers cause two different nozzle problems. Keep them apart: the usual workshop rule lumps them together.

By size, a filler clogs. A particle or clump close to the size of the orifice can lodge across it and block it. That is why a 0.2 mm nozzle is ruled out for marble, sparkle and glow. Bambu Lab, for example, warns about it on its 2024–2025 datasheets ("not recommended… may clog"), and lists only 0.4, 0.6 and 0.8 mm for its wood PLA and its glow filament. Wood clogs most, because its fibers bunch up and char; with wood, 0.6 mm is the safe bet.

By hardness, it wears. The strontium aluminate in glow filament is far harder than brass and opens up the orifice. Mineral fillers and flakes vary by brand, and many of them wear brass too. Glass microspheres are hard but round and fine: they barely wear, and Bambu allows its PLA Galaxy down to 0.2 mm. Wood flour is soft: it clogs, but it does not wear.

WoodClogFlakes (sparkle)Flakes lying along thebeadMineral (marble)WearGlowFast wear: enlargedorificeSize → clogHardness → wear
Each filler mostly causes one of the two problems: size clogs, hardness wears. Flakes lie down along the flow.

For marble, sparkle and glow, use a hardened nozzle, preferably 0.6, and never 0.2; hardened steel needs 5–10 °C more or 10–20 % less flow (Nozzles: size and material). Glow is the extreme case: Prusa rates its surface-hardened INDX nozzle at 0.5 kg of glow filament, against 10 kg of PETG-CF. Not every brand uses the same filler (some "marbles" use soft fillers); when the datasheet does not say, treat the filament as abrasive. Wood is not on that list: brass is fine for it; its problem is clogging.

Wear gives no warning. A worn orifice lays beads wider than you calibrated for, and the calibration stops being valid without the printer telling you. An abrasive filler is as hard on everything upstream of the nozzle: it scores PTFE tubes and extruder gears, and Bambu advises against running its Glow through the AMS Lite.

The datasheets for decorative PLAs give 190–230 °C (190–240 °C for wood), and Bambu's general table for PLA with abrasive filler gives 210–240 °C. With a hardened nozzle, stay in the upper half: 210–230 °C. The 35–45 °C bed on the datasheets is for a cool plate; on PEI, use 45–65 °C.

The filler costs strength. Figures from one manufacturer, on specimens printed and dried at 55 °C for 8 h as each datasheet specifies:

Tensile strength of decorative PLAs (Bambu Lab datasheets)
Filament XY (MPa) Z (MPa) Z/XY Elongation at break XY / Z
PLA Basic (reference, datasheet V2.0) 39 35 90 % 12.2 / 7.5 %
Marble 42 36 86 % 6.7 / 5.3 %
Sparkle 39 32 82 % 11.7 / 6.8 %
Glow 32 26 81 % 8.6 / 6.5 %
Microspheres (Galaxy) 26 21 81 % 9.3 / 7.1 %
Coextruded dual-color silk (Silk Dual Color, datasheet V3.0) 27 18 67 % 3.5 / 1.7 %
Wood 26 15 58 % 15.3 / 4.5 %

The decorative rows come from V1.0 datasheets (dual-color silk from V3.0), so the Basic row is its V2.0 sheet, the nearest test series; V3.0 gives other figures. Mineral fillers keep the across-layer ratio (81–86 % against 90 % for Basic), though some lower absolute strength: Galaxy reaches 26 MPa against 39. Wood and coextruded silk lose a lot between layers. HDT at 0.45 MPa sits around 55–60 °C for all of them, as for PLA, so under load they work up to about 40 °C (Heat, cold, sunlight and chemicals). If it also has to carry load, print the structure in plain PLA or PETG and only the visible body in the decorative filament (see Designing for multicolor), or orient it so the load runs along the layers.

They dry like PLA: 45–55 °C for 8 h. Bambu's datasheets for wood, marble, sparkle and Galaxy ask for 55 °C for 8 h and storage below 20 % relative humidity. Wood flour absorbs water in its own right, and a damp wood spool strings and crackles more than plain PLA. Drying times are in Drying and storing filament.

Wood

This is PLA with wood flour. The percentage varies by brand and can almost never be checked, so do not trust the figure on the label. Its density is 1.21 g/cm³, close to PLA's: it weighs far more than the wood it imitates and sounds like plastic.

Bambu's datasheet gives 190–240 °C, 0.6–1.0 mm of retraction on a direct-drive extruder, speed below 250 mm/s, and textured PEI, or smooth PEI with a glue stick, which here acts as a release agent.

It clogs for a physical reason: wood fibers do not melt; left in the heat, they char. The typical clog follows a pause, a long travel move or a spell with the hotend idling at temperature. Wood that sits still in the nozzle turns into a charred plug, and the next print starts with a partial clog. To avoid it:

  • No 0.2 or 0.25 mm nozzles; 0.6 mm is better.
  • Do not leave the hotend hot with wood inside.
  • When you finish the spool, purge a few centimeters of plain PLA.
  • Keep retraction short: a long retraction pulls molten material up into the cold zone.

Temperature controls color: the hotter, the darker, because the wood toasts more. Change the nozzle temperature at chosen layers and you get bands like the rings of a trunk. Bambu Studio, OrcaSlicer and PrusaSlicer let you do this from the preview, with custom G-code at the layer you pick. Stay inside the datasheet range, and expect each change to take a few layers to show fully.

It sands well, from coarse grit to fine, and takes stain or oil better than plain PLA because the exposed fibers soak it up. Under varnish it looks like MDF, not solid wood. For finishing, see Sanding and smoothing and Painting and priming.

It is the weakest in the table: 15 MPa in Z, 58 % of the XY figure, and only 4.5 % elongation between layers. Never use it for a snap-fit, a hook or a thread.

Marble, stone and speckle

This is PLA with mineral particles in a color that contrasts with the base: each speck is one particle. The datasheet gives 190–230 °C and a 35–45 °C bed, with no 0.2 mm nozzle. The surface comes out matt because the particles scatter light, so it hides layer lines the way matt PLA does; PLA and its variants explains the mechanism.

How it looks depends on the scale of the part. A speck is always the same size, so a 3 cm figure looks like coarse granite and a 30 cm vase like fine-grained stone. Choose it for medium and large parts.

Sanding brings more particles to the surface and makes the part look more like stone, and it does not clog the paper the way plain PLA does.

It is slightly stronger than Basic (42/36 MPa against 39/35), but more brittle: 6.7 % elongation in XY against Basic's 12 %.

Sparkle and microspheres

Two different fillers are sold under this name. The first is metal or mica flakes; Bambu describes the filler in its Sparkle as "metallic particles". Flakes are flat, and the shear flow inside the nozzle lays them down along the bead, like logs in a river. That is why they glint on walls and on top layers facing the light, and why the glint depends on the direction of the bead. Ironing or a slow top layer leaves the top surface flatter and changes the sparkle: try it on a coupon.

Large flakes clog small orifices: no 0.2 mm with Sparkle. They also wear, so use a hardened nozzle: the brand's own compatibility list recommends 0.4, 0.6 or 0.8 mm hardened steel.

The second filler is glass microspheres, the one behind the galaxy effect (PLA Galaxy). They are smaller and smoother, and Bambu allows 0.2 mm. The melt is more viscous, though: a melt flow index of 11 g/10 min against Basic's 42. Print it slower or hotter.

Both hide layer lines because the eye reads the glints, not the steps. They are a good choice for domes, for parts with very visible stair-stepping, or for parts printed with thick layers. Looking like metal does not mean they polish like metal; that belongs to Metal filaments and sintering.

Glow in the dark

It glows because its filler is a photoluminescent pigment: it stores energy from ultraviolet or blue light and releases it slowly. Today that pigment is strontium aluminate; older products used zinc sulfide. Charge it with sunlight, a UV LED or a bright white LED. It is brightest in the first few minutes and fades over a few hours; how long it lasts depends on the product and on how long it was exposed.

Three things make it glow brighter:

  • More material between the light and the eye. Thicker walls and more perimeters: a part with 2 walls glows less than one with 4. The effect saturates at around 1–2 mm of thickness; beyond that it gains nothing.
  • A light base underneath. A dark background absorbs the light it emits.
  • The pigment loading, which varies by brand.

It prints like PLA (190–230 °C per the datasheet, a 35–45 °C bed on a cool plate, under 250 mm/s), with a hardened nozzle and never 0.2 mm. Bambu's shop leaves no doubt: for regular use, a hardened nozzle is required. If your machine has several nozzles, keep one hardened nozzle for glow.

It works best for details: a logo or a clock face a few layers thick on a plain body. Put it on top faces or outer walls, where the light reaches it. How to divide filaments within a part is in Designing for multicolor.

Translucent and "transparent"

Set your expectations first: FDM does not print parts that are clear like glass. The spool is clear; the part comes out translucent. Light scatters at every boundary it crosses, and a printed part is full of boundaries. A pane of glass has only two: the front face and the back. A print has the boundary between every pair of beads, the ridges on the surface, and the small air gaps the toolpath leaves between beads. Prusa sums it up: bubbles scatter light inside the object.

Standard settingsAir gapsOuter ridgesScattered lightSettings for clarityMostly straight light1231More flow: gaps closed2Hot and slow: beads fused3Coating: ridges filled
Light scatters at every gap and every boundary between beads. Closing the gaps, fusing the beads and filling the ridges lets it through straighter.

Gaining clarity means removing boundaries and gaps; every setting follows from that (starting points):

  1. Over-extrude slightly to close the gaps. Prusa's example: a flow ratio of 110 % and more overlap between infill and walls.
  2. Print hot and slow so the beads fuse instead of stacking.
  3. With PETG, turn the part-cooling fan down (Prusa goes as far as switching it off) so each bead flows into its neighbor.
  4. Use fewer, wider beads where the shape allows: a single-wall shell in vase mode, or 100 % solid infill with the lines aligned.
  5. Dry the filament. A damp spool foams, and every bubble scatters light. PETG takes up enough water to bubble: dry it at 60–65 °C for 8 h before a translucent part.

In practice, PETG and PCTG come out clearer than PLA; the material is covered in PETG, PCTG and other copolyesters. "Translucent" PLA gives a frosted look that suits lampshades and diffusers.

The outer ridges scatter as much as the inside. Wet-sand to a fine grit and finish with clear varnish or epoxy, and you fill the ridges and reach the most clarity a printed part allows (Coatings and epoxy). If you need a lens or a visor that is genuinely clear, print it in resin or buy it: FDM or resin for your part.

A diffuser is the easy case: there the frosting is what you want. Lithophanes and color through thickness are in Painting with filament and light.

Dual- and tri-color coextruded

Two (or three) colors are extruded side by side in a single strand, almost always with a silk finish. The halves do not mix in the nozzle because at these speeds the melt moves in laminar flow; at higher temperatures the colors start to blend at the boundary. Every bead you lay has color A on one side and color B on the other.

On a round part, one side comes out in one color and the opposite side in the other. The filament barely twists on its way to the nozzle, so half A points at the same side of the machine for the whole print. The color you see on a wall depends on which way that wall faces, not on the direction the nozzle travels. On a cylinder, the face toward A's side comes out in color A, the opposite face in B, and the two faces in between show a blend band. On the top face you see both halves of every infill line, so it comes out striped.

Coextruded filamentColor AColor BLaid beadNozzle pathBlend bandA always faces the same side of the machineStripes on the top faceVase mode: one wall, no seam
Half A always faces the same side of the machine: on a cylinder it shows on the half of the outline facing that side, and the top face comes out striped.

In the slicer and on the machine:

  • Vase mode for the cleanest effect: a single outer wall, with no seam and no changes of path.
  • A short filament path. If the filament twists in a long tube or a filament switcher, the line between the colors rotates with height and swirls; several brands warn about this. It comes from the filament path, not from a setting, and it does not always go away entirely.
  • Orientation. Faces pointing at the same side of the machine always come out in the same color: rotate the part on the plate so the face that will be seen points toward the color you want.

Underneath, it is still a silk PLA: it inherits silk's mechanics (18 MPa in Z, 67 % of XY) and its rules for shine. A hotter, slower outer wall shines more; start at around 30–60 mm/s. Why silk shines: PLA and its variants.

Do not confuse coextruded filament with gradient or rainbow spools, where the color changes along the length of the filament. With those, the height of each band depends on how much filament each layer uses. An example: a single-wall vase 100 mm across, with a 0.45 mm wide bead and 0.20 mm layers, uses π × 100 ≈ 314 mm of outline times 0.45 × 0.20 = 0.09 mm² of cross-section, about 28 mm³ per layer. 1.75 mm filament has a 2.4 mm² cross-section, so that is about 12 mm of filament per layer. A 1 m color section covers about 85 layers: about 17 mm of height. A solid part uses far more per layer, and its bands come out thinner. The length of each section is set by the manufacturer.

One profile per filament

Create a profile for each decorative filament, even ones from the same brand. On one manufacturer's datasheets, the melt flow index runs from 11 (Galaxy) to 34 (Sparkle) g/10 min, against Basic's 42, so the flow ratio and the maximum flow change. Run the tests in Flow ratio and max flow tests.

When it fails

Symptom, cause and fix
Symptom Cause Fix
Partial clogs with wood Wood charred after idling hot or a long retraction 0.6 mm nozzle, short retraction, purge with PLA when done
Wider lines and fits that stop fitting after a spool of glow Worn brass orifice Hardened nozzle and recalibrate
Dull silk or dual-color Outer wall too fast or too cold Slower outer wall, 10 °C hotter
Cloudy "transparent" part Gaps, damp spool, fan too high Dry the spool, raise the flow, lower the fan
Dual-color split swirls Filament twists on its way to the nozzle Shorter filament path, vase mode
The color you wanted ends up on the back face The visible face points at the other color's side Rotate the part on the plate

How to test it

Before the real part, print a small coupon of the visible face. The look depends on the toolpath and on scale (the direction of the glint, the dual-color split, the size of the speck), and a coupon shows it to you in minutes. Test coupons explains how to design one.

See also

Design it in KapyCAD

Size the walls, the clearances and the orientation for the material you chose.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?