The bottle says "standard", "ABS-like", "8K", "tough" or "water-washable". Only some of those words tell you what the cured part can take; the rest describe how it prints or how it washes. Telling them apart is the first step in choosing a resin, and the second is reading three figures on the datasheet: elongation at break, HDT and impact. Across families one trade-off cannot be dodged: the resin that bends does not take heat, and the one that takes heat snaps. Choose by what would break your part and, if it needs both, take it out of resin.
What a cured resin is
Every desktop resin is a liquid of acrylate or methacrylate monomers and oligomers with a photoinitiator. Under 405 nm light on consumer printers (some professional and dental machines use 385 nm), those molecules cross-link into a thermoset: it will not melt or reshape the way a thermoplastic does. The families differ in how long and flexible the chains are between cross-links. Short chains give a dense network: the part comes out stiff and heat-resistant, but brittle. Long chains give a loose network: the part comes out tough or rubbery, but softens with little heat.
What the label tells you, and what it does not
Names that describe properties refer to the cured part: standard, ABS-like, tough, nylon-like, flexible, elastic, high-temperature, rigid or ceramic-filled. But "ABS-like" is not a standard. It guarantees no minimum elongation, impact strength or HDT, and one "ABS-like" bottle may stretch several times further than another before it breaks. Read the datasheet, not the name.
The process names say nothing about strength. "8K" or "high resolution" means a formulation tuned so light does not spill past small pixels, with more UV absorber and a finer pigment. "LV" (low viscosity) only says it flows better. "Low odor" or "plant-based" resins are still acrylates and equally sensitizing: the gloves and ventilation in Handling resin safely still apply. "Water-washable" changes the washing chemistry and has its own section below. Nor does the wavelength separate desktop brands: every consumer MSLA resin cures at 405 nm. Even so, in late 2026 some professional systems use their own cartridges and settings, and a resin made for one may need the open-material mode and a fresh calibration on another.
Three datasheet values usually decide it:
- Elongation at break: whether the part bends or snaps. Below roughly 10 %, it snaps.
- HDT (heat deflection temperature) at 0.45 MPa: the temperature at which it deforms under a light load.
- Notched Izod impact: how hard a blow it survives at a notch.
Shore hardness only matters for flexible resins. What each number measures and how it is tested is in Reading a material datasheet and Stiffness, strength and toughness.
Those values are measured on test bars post-cured exactly as the datasheet specifies: time, light and temperature. An under-cured part is softer and more flexible, but also weaker and tacky. An over-cured standard resin becomes more brittle and can crack. So comparing two brands only makes sense with the same test standard and the same cure. With high-temperature resins, the cure changes everything (you will see why in their section).
Standard resin
The default resin: the cheapest, and the one with the finest detail. Elegoo Standard's datasheet gives 34 MPa tensile strength, 8.8 % elongation at break, Shore D 80 to 88 and a notched Izod of about 24 J/m. On paper it matches PLA (35 MPa); in practice it snaps cleanly at notches and thin sections, because it barely deforms before it breaks.
On heat, standard resins sit around 55–62 °C HDT at 0.45 MPa, when the maker publishes the figure: Formlabs Grey V5 states 62 °C with its default cure. Many desktop brands do not publish it. Assume PLA's HDT (57 °C) or a little less.
Sunlight and UV keep curing it. Outdoors it yellows, clear resin most of all, and turns brittle. Unpainted, it will not last outdoors.
This is the resin for miniatures, scale models, masters for silicone molds, look-and-fit prototypes, and dental or jewelry study models. Keep it away from clips, snap-fits, threads that get tightened and anything that might be dropped.
ABS-like, tough and nylon-like resins
Same chemistry, with longer, more flexible chains and impact modifiers. Stiffness (the modulus) drops, elongation rises sharply; the price is slightly softer detail and higher viscosity.
| Resin | Tensile strength | Elongation at break | HDT | Notched Izod |
|---|---|---|---|---|
| Siraya Tech Blu | — | 32 % | 70 °C (0.45 MPa) | 45 J/m |
| Siraya Tech Blu Nylon Black | — | 50 % | 63 °C (0.45 MPa) | — |
| Siraya Tech Blu Nylon Mecha White | 58 MPa | 37 % | 65 °C (0.45 MPa) | — |
| Siraya Tech Tenacious | — | ~70 % | 55 °C (0.45 MPa) | 57 J/m |
| Formlabs Tough 1500 V2 | — | 155 % | 66 °C (per Formlabs) | — |
"—": the datasheet gives no figure, or it could not be verified. Desktop tough resins land between 25 and 70 % elongation. Engineering grades such as Tough 1500, which Formlabs sells as "PP-like", go past 150 %. Their HDT, on the other hand, stays within 55–70 °C. An "ABS-like" resin is not ABS: ABS filament reaches 87 °C HDT and usually stretches further.
A tough resin gives you impact and flex, never temperature.
Use it for clips and snap-fits with small deflections (the limits are in Print-friendly snap fits), housings that might get dropped, functional prototypes and board-game pieces with thin spears that must not snap. Under constant load it creeps more than ASA or PC, as Creep and fatigue explains.
On the printer it needs more exposure than standard and is more viscous, so it prints better with a slower peel or a heated vat (How a resin printer works). Fresh off the plate it is softer, and its supports bend before they let go (Orienting and supporting resin prints).
For miniatures, a common trick is to add 10–30 % of a tough or flexible resin, such as Tenacious, to standard so parts break less. It works, but nobody has measured that blend: no datasheet applies to it, and you have to repeat the exposure test.
Flexible and elastic resins
These are rubbery networks, and their hardness is measured in Shore A, like TPU. Per Formlabs' datasheets, Flexible 80A V2 (80 A) stretches 230 % before breaking and Elastic 50A (50 A) 160 %. Desktop brands sell very different hardnesses under the "flexible" label, from Shore A to Shore D: check the hardness before the name.
They tear where TPU would not. Elongation is high, but tear strength at a notch or a support mark is low, and a small nick becomes a tear. Design without sharp inside corners, and cut the supports off rather than pulling them.
On the plate, the fresh part is soft, sags and sticks to the film. It needs thicker supports and more exposure. Under-cured, the surface stays tacky. Wash it no longer than necessary: isopropyl alcohol makes it swell.
It suits prototype gaskets and living hinges, soft-touch grips, cushioning and molds for small casts. For a flexible part that has to last, see TPU and flexible filaments: FDM TPU is tougher and resists tearing far better. Flexible resin only wins on detail.
High-temperature and filled rigid resins
Here the network is short and dense, and rigid grades also carry a glass or ceramic filler. They gain HDT and stiffness at the cost of minimal elongation, 1 to 3 %. Per their datasheets, Formlabs High Temp reaches 238 °C HDT at 0.45 MPa. Glass-filled Rigid 10K gives an 11 GPa modulus and 218 °C with its thermal post-cure. Among desktop resins, Phrozen TR250LV is rated at 80 °C.
Those figures depend on three different cure states:
- Fresh off the printer: High Temp is around 49 °C, Rigid 10K about 65 °C.
- Hot UV cure at 60–80 °C, as the datasheets ask: High Temp rises to about 142 °C and Rigid 10K to about 163 °C. TR250LV, with its UV cure alone, stays at 62 °C.
- With a thermal post-cure in an oven: 238 °C for High Temp, 218 °C for Rigid 10K, 80 °C for TR250LV after an hour at 100 °C.
The HDT on the bottle is only reached with the datasheet's thermal post-cure. A consumer wash-and-cure station does not heat the part in a controlled way: it does not even reproduce the second state. A heated curing chamber such as the Form Cure (up to 80 °C) does reproduce it, but it does not do the oven thermal post-cure either, and without that the part ends up far short of the bottle's figure.
They are the most brittle resins on the market, by design: the dense network that takes the heat is the one that snaps. Their place is hot parts that take no knocks and no bending: molds for low-temperature casting or thermoforming, fixtures for hot air or fluids, parts near a heat source. No clips, and nothing that might be dropped.
Filled grades settle in the bottle. Shake the bottle and stir the vat thoroughly before every print.
Water-washable resin
What changes: before curing it disperses in water, so you wash it in tap water instead of isopropyl alcohol. Once cured, its properties are those of a standard resin: a typical datasheet gives 30–35 MPa and 6–9 % elongation.
What does not change: it is still a sensitizing acrylate, and the rinse water is contaminated with uncured resin. Cure that water before you throw it away, and never pour it down the drain. The procedure is in Handling resin safely.
The monomers that make it washable attract water, and the cured network goes on absorbing moisture and swelling. So a long soak, or curing a part while it is still damp, leaves stresses that end in cracks. Do not leave parts soaking longer than the datasheet says (eSUN, for one, advises against long washes), and dry them completely before post-curing. Over-cured, it turns brittle and cracks; the datasheet warns about this. Washing and curing times are in Washing and curing resin parts.
It does the same job as standard when you do not want alcohol on the bench. It is not a "safe" or "eco-friendly" resin.
Castable resin for metal casting
You print the pattern, embed it in investment (a plaster-based casting compound), burn it out in a kiln and pour metal into the cavity. The resin must leave no ash and must not expand enough to crack the investment.
There are two kinds. One is wax-filled formulations: Formlabs Castable Wax carries 20 % wax, and other makers load more. The other is low-ash photopolymers, such as Formlabs True Cast. Either way, the stated ash stays below 0.1 %. A standard resin expands and leaves residue as it burns: it cracks the investment and the casting comes out with inclusions.
Each castable resin comes with its burnout cycle in the datasheet, with its ramps and holds. Follow it to the letter. High-wax grades are softer: handle them with care.
Typical uses are rings and other jewelry, dental frameworks and small metal art pieces. For larger metal parts, see When to order the part instead.
Specialty resins
- Clear: clear resins are only truly clear after sanding and polishing or a coat of lacquer (Coatings and epoxy), and they yellow with UV and time.
- Dental and biocompatible: they are certified only within a validated workflow, with a specific printer, wash and cure. The same bottle in another process is not certified, and none of that makes them food-safe (Printing for food contact).
- TPO-free: the EU classified the photoinitiator TPO as toxic for reproduction, category 1B, and as a result banned it in cosmetics from 1 September 2025. Hence the new "TPO-free" lines. The mechanics do not change; the safety data sheet does (Handling resin safely).
Choosing by what the part has to withstand
The logic is the same as with filaments: start from what would break the part.
- Detail and light loads → standard or water-washable.
- Knocks, clips or bending → tough, ABS-like or nylon-like.
- Behaving like rubber → flexible or elastic.
- Above about 70 °C, no knocks → high-temperature, with its full thermal post-cure.
- A pattern for casting → castable.
If it needs heat resistance and toughness together, or will sit in the sun, resin is the wrong process: go back to FDM or resin for your part.
| Family | Elongation at break | HDT at 0.45 MPa | Typical part | Avoid for |
|---|---|---|---|---|
| Standard / water-washable | 6–9 % (Elegoo Standard 8.8 %) | ~55–62 °C (Formlabs Grey V5: 62 °C) | Miniatures, scale models, mold masters | Clips, threads, parts that get dropped |
| Tough / ABS-like / nylon-like | 25–70 % (Siraya Tech Blu 32 %), over 150 % (Tough 1500) | 55–70 °C | Clips, housings, functional prototypes | Heat, constant load |
| Flexible / elastic | 160–230 % (Elastic 50A, Flexible 80A) | Not applicable | Gaskets, grips, cushioning | Tearing, long-term use |
| High-temperature / filled rigid | ≈1–3 % | 80 °C (TR250LV) to 238 °C (High Temp), only with thermal post-cure | Molds, hot fixtures | Knocks, bending |
| Castable | Not applicable | Not applicable | Jewelry and dental patterns | End-use parts |
When it fails
| Symptom | Cause | Fix |
|---|---|---|
| A standard-resin clip snaps the first time you use it | It needed more elongation than standard's 8.8 % | Reprint it in tough resin, redesign it so it does not deflect more than the resin allows, or move it to FDM |
| A "high-temperature" part warps in a car parked in the sun | It never got its datasheet's thermal post-cure, or the resin cannot take that temperature | Redo the full cure or change process |
| A tough part slowly bends on a warm shelf | That is what to expect from 55–70 °C HDT under constant load | Print it in ASA or PC |
| A flexible part tears at a support mark | The mark acts as a notch, and flexible resin has little tear resistance | Cut the supports instead of pulling them, and round the inside corners |
| A water-washable part cracks days later | It was cured damp or over-cured | Dry it completely and cure only as long as the datasheet says |
See also
- Orienting and supporting resin prints: how to orient the part and which supports each family needs.
- Washing and curing resin parts: the wash and cure times that set the datasheet's properties.
- FDM or resin for your part: what to do when the part needs heat resistance and toughness at once.
- Handling resin safely: gloves, ventilation and waste, whichever resin you use.