Before you choose a printer, a material or an orientation, decide which process will make the part: each one builds in its own way and favors its own geometry. Anyone printing at home or in a small workshop will meet five: FDM, resin, powder sintering (SLS and MJF), metal and pellets. All five make sense once you answer two questions: how does the material get into place, and what holds the part up while it grows? Those two answers tell you what you can print on your desk and what is better ordered out.
Two questions that sort every process
They are all additive manufacturing: they add material layer by layer from a sliced model, whereas a milling machine removes it. From there they part company.
How is the material placed? There are three answers: a nozzle that moves and draws (FDM and pellets); light that cures a layer of liquid (resin); energy that melts a chosen area of a thin layer of powder (SLS, MJF and metal). The difference shows up in print time. A nozzle is limited by how fast it can lay down plastic: a current FDM printer melts about 21 mm³/s of PLA in practice (Volumetric flow sets the speed). A process that exposes the whole layer at once, such as MSLA resin or MJF, takes the same time per layer for one part as for twenty, so filling the volume barely lengthens the print. In SLS and metal the laser traces the cross-section, so time grows with the area melted, but spreading each layer of powder costs the same for the whole batch.
What holds the part up while it grows? In FDM and pellets, every bead has to rest on something already printed: hence overhangs and supports. In resin the part hangs upside down from the plate, and every island needs its own support. In a polymer powder bed, the unfused powder holds the part, so there are no supports. In a metal powder bed the part is welded to the plate and carries supports anyway, to anchor it against warping and to carry the heat away. This second question is why SLS can fill the volume with parts nested on top of one another, including interlocking parts that rest on nothing, and FDM cannot.
The ISO/ASTM 52900 standard sorts additive manufacturing into seven categories. The five processes here belong to three of them: material extrusion, vat photopolymerisation and powder bed fusion; metal adds a fourth, binder jetting. The other three are summed up at the end.

FDM: a nozzle that draws in molten plastic
A motor pushes 1.75 mm filament into a hotend, and a 0.4 mm nozzle lays down a squashed bead about 0.45 mm wide and 0.20 mm tall, path by path, layer by layer. What that means for your design is covered in How FDM shapes your design.
It is the process with the widest range of materials within a hobbyist's reach: PLA, PETG, ABS and ASA, polycarbonate, nylon, TPU and the fiber-filled grades; add a filament switcher and it prints in several colors. To choose between them, read Choosing a filament.
The part comes out tough and cheap, but anisotropic. Each layer welds to the one below after that one has partly cooled, and that bond is the weak plane. For design, assume the part is half as strong in Z as in XY, or 30 % if the material is fiber-filled, and orient it so the main load runs along the beads (Layer adhesion and anisotropy). The layer lines show, and the 0.45 mm bead sets the limit on detail. Speed is limited by flow, not by motion.
It is the cheapest machine and the cleanest to run: an enclosed CoreXY or a modern bedslinger will print for hours without you stepping in. That does not make it safe to leave alone. What should keep watch over it, starting with a smoke detector, is covered in Fire risk and unattended printing. Clean does not mean harmless either: every FDM print gives off ultrafine particles and volatile compounds, so never print in a bedroom, and when the print ends leave the printer closed with the filter running for 10 to 20 minutes before opening it (Emissions and ventilation).
That makes it the process for functional parts (brackets, housings, jigs, mechanisms, prototypes, anything that has to carry a load or flex in a snap-fit) and the one the rest of this book focuses on.
Resin: light cures a whole layer at once
In an MSLA printer, the usual kind on a desk, the part hangs upside down from a plate dipped into a vat of photopolymer. Light from an array of UV LEDs shines through an LCD screen that masks it to the shape of the layer, and cures a sheet 0.025 to 0.1 mm thick (0.05 mm is typical) against a clear FEP film. The plate rises, the film peels away and the cycle repeats. Laser SLA and projector DLP machines do the same job with a different light source. The mechanism is explained in depth in How a resin printer works.
XY resolution is set by the pixel size, not the bead width. As of late 2026, a 16K desktop screen such as the one in the Elegoo Saturn 4 Ultra 16K has pixels of about 14 × 19 µm. Professional machines such as the Formlabs Form 4 use pixels of about 50 µm, with antialiasing to smooth the edges. The 16K pixel is about 25–30 times narrower than a 0.45 mm FDM bead, but reliable detail spans several pixels: in practice, resin resolves XY detail about ten times finer than FDM, with 0.025–0.05 mm layers against 0.20 mm. That is why 28 mm miniatures and jewelry models are printed in resin.
The part comes out smooth and, after post-curing, nearly isotropic: each layer cures on top of the one below and forms a single chemical network with it, instead of being welded to it afterwards. Before post-curing that network is only half formed, which is the physical reason post-curing is not optional. How brittle the part is depends on the resin. Standard resins are brittle next to FDM plastics; tough and engineering resins narrow the gap without closing it. Many also creep under sustained load and yellow with UV and heat. The differences are in Types of resin.
You pay for all this in handling: liquid resin is never touched without nitrile gloves, IPA is flammable and nothing goes down the drain (Handling resin safely). Every part is washed and post-cured under UV, and supports leave marks. The build volume is smaller than on FDM: a 10-inch machine, the most common size, offers about 210 × 120 × 220 mm, and 14- to 16-inch machines reach about 300 × 165 × 300 mm.
It is used for miniatures, figures, dental and jewelry work, prototypes with fine detail, and small parts where finish and detail matter more than toughness.
SLS and MJF: the part grows buried in powder
In selective laser sintering (SLS), a roller spreads a 0.1 mm layer of nylon powder over a bed heated to slightly below its melting point. A laser traces the part's cross-section and sinters the particles, the bed drops and the cycle repeats. The finished block cools for hours before the parts are dug out and blasted clean. A benchtop SLS printer such as the Formlabs Fuse 1+ 30W works with layers of about 0.11 mm in a 165 × 165 × 300 mm chamber.
In HP's Multi Jet Fusion (MJF), the powder bed is the same, but there is no laser. A print head jets a fusing agent where the part goes and a detailing agent along its edges, and an infrared lamp sweeps the whole layer. The treated areas absorb the heat and fuse, the whole layer at once, in layers 0.08 to 0.09 mm thick. On large batches it is faster and more consistent than a laser. Parts come out gray and are nearly always dyed black.
No supports are needed because the unfused powder holds every part in place. You can fill the whole volume in three dimensions, with parts nested on top of one another, and print chains, hinges and pre-assembled mechanisms without supports and without designing them to sit on the bed, as FDM demands. You can also make internal channels, as long as the powder can get out: a hollow resin or powder part needs at least two drain holes at opposite ends; FDM does not (Designing for resin).
The part is nylon (PA12 or PA11, also glass- or carbon-filled), TPU or, in MJF and at some services, polypropylene. It is tough, nearly isotropic, and has a matt, grainy surface that feels like fine sandpaper. For living hinges that must survive thousands of cycles, PP and PA11 outlast PA12. As a guide, services work to tolerances of about ±0.3 % (no tighter than ±0.3 mm) and minimum walls of 0.7 to 1.5 mm depending on the service. Each service's figures are covered in When to order the part instead.
Even a complete benchtop SLS setup, with printer, powder station and blasting cabinet, costs more than ten times as much as a good FDM printer. It needs its own corner of the workshop with extraction, and handling the fine powder calls for an FFP2 mask and thorough cleaning. Unfused powder degrades with heat and has to be blended with fresh powder for every run. That is why nearly everyone orders SLS and MJF parts from a service: short runs of functional nylon parts, snap-fits and living hinges that have to survive many cycles, ducts, complex parts that would need a forest of supports in FDM, and print-in-place assemblies.
Metal: melt the powder or sinter a filled plastic
Laser powder bed fusion of metal (LPBF; services call it DMLS or SLM) fully melts layers of metal powder 0.02 to 0.06 mm thick in a chamber of inert gas. The usual materials are 316L or 17-4PH stainless steel, AlSi10Mg aluminum, Ti6Al4V titanium, tool steel and nickel superalloys (such as Inconel 718 or 625). Here the powder does not hold the part up. The part is welded to a thick steel plate and carries supports, because the melt pool shrinks hard as it solidifies and would curl the part until it tore free. Next comes a stress-relief heat treatment with the part still on the plate; then it is cut off with wire EDM or a band saw, the supports are removed by hand or by machine, and the critical faces are often machined.
The part is dense metal, with static strength close to that of wrought material after heat treatment, and it comes out with a rough surface. Fatigue strength stays lower unless the part is hot isostatically pressed (HIP) and its surfaces machined, because residual porosity and roughness start cracks. The machines are industrial, and so is the powder: fine aluminum and titanium powder is reactive and can burn or explode if it is dispersed in the air. For a hobbyist, LPBF is something you order.
Binder jetting glues metal powder layer by layer with a print head. The "green" part is then sintered in a furnace, where the binder burns off and the part shrinks. It lowers the cost per part in production runs, but makes little sense for one-offs.
At home, the route is bound metal filament: 87–90 % metal powder by weight in a polymer binder. You print it on your FDM machine and send it off to have the binder removed (debinding) and the part sintered, unless you have your own controlled-atmosphere furnace, because 316L steel sinters above 1300 °C in argon or hydrogen. The part turns into solid metal and shrinks by 13 to 20 % in every dimension. It is the same sequence as metal injection molding (MIM): green part, brown part, sintering. Do not confuse it with metal-filled PLA, which is heavier and shines when polished, but is still plastic. The whole process is covered in Metal filaments and sintering.
Printing in metal pays off where a cutter cannot reach and the price per part justifies it: brackets, manifolds, heat exchangers, mold inserts and parts lightened by topology optimization.
Pellets: FDM without filament
A screw extruder, like a small injection barrel, is fed with pellets: the same plastic granules that filament and injection-molded parts are made from. The screw melts them and meters them through the nozzle. The motion system and the layer logic are those of FDM; only the feed changes. The process is called FGF (fused granular fabrication) and, at large scale, LFAM.
It exists for two reasons: flow and material cost. A desktop hotend at 21 mm³/s of PLA lays down about 0.1 kg/h. Benchtop pellet machines claim around a kilo per hour (a manufacturer figure), with nozzles several millimeters across. Industrial gantry and robot-arm systems print furniture, molds and plugs for boat hulls. Pellets cost less per kilo than filament, and there are grades, and shredded recycled material, that are never sold as filament.
The part has FDM's traits at a larger scale: beads millimeters wide, thick layers, strong anisotropy, and on large parts often a machining pass afterwards. Pellets need drying like filament, usually in a hopper dryer right before printing and throughout the run.
A benchtop pellet printer costs several thousand euros and is a workshop machine. For someone printing at home it does not pay off yet; it does for large parts, molds and tooling, research with your own compounds, and workshops that print tens of kilos a week. The recycling side is covered in Printing with less waste.
The five processes side by side
| Process | How it makes a layer | Typical layer | Finest XY detail | Supports | Materials | Character of the part | Where it is made |
|---|---|---|---|---|---|---|---|
| FDM | Nozzle drawing beads | 0.20 mm | Bead ≈0.45 mm | Overhangs beyond ~45° | PLA, PETG, ABS/ASA, PC, nylon, TPU, fiber-filled | Tough, anisotropic, layer lines | Your desk |
| Pellets | Screw and coarse nozzle | Millimeters | Bead millimeters wide | As FDM | Pellets in many grades, recycled | Large, coarse, very anisotropic | A workshop |
| Resin (MSLA) | UV light through a screen, whole layer | 0.025–0.1 mm (0.05 typical) | 14–50 µm pixel | Always | Standard, tough and engineering photopolymers | Smooth, nearly isotropic, brittle to tough | Your desk |
| SLS / MJF | Laser, or agent and infrared, on powder | SLS 0.1–0.11 mm · MJF 0.08–0.09 mm | Walls of 0.7–1.5 mm | None | PA12, PA11, filled grades, TPU, PP | Tough, nearly isotropic, matt and grainy | A service |
| Metal (LPBF) | Laser melting metal powder | 0.02–0.06 mm | Walls of tenths of a millimeter; rough surface | Always; the part is welded to the plate | Stainless, aluminum, titanium, tool steel, nickel superalloys | Dense metal after heat treatment | A service |

Which process for your part
Ask yourself three questions, in this order.
- Does it have to carry a load, flex or take knocks? FDM or SLS/MJF. PETG, nylon, TPU and sintered nylon bend before they break; PLA is stiff but brittle, especially across the layers. Resin only if it is an engineering resin.
- Does it need detail below about 0.3 mm, or a smooth surface without sanding? Resin: the detail is about ten times finer than FDM.
- Is it complex, nested or interlocking, or do you need dozens of copies in nylon? SLS or MJF from a service: the powder holds it up without supports and every run uses the whole volume.
Move to metal only when plastic cannot take the load or the temperature. Move to pellets only when the part is measured in tens of centimeters and in kilos.
The everyday decision, FDM or resin, is covered in FDM or resin for your part. When to order SLS, MJF, resin or metal, and how to prepare the file, is explained in When to order the part instead.
The other three families
That leaves three categories of the standard worth recognizing. Material jetting deposits droplets of photopolymer that are cured with UV, in full color and in several materials, and is almost exclusively industrial. Directed energy deposition melts metal wire or powder with a laser or an arc to repair or build large metal parts. Sheet lamination cuts and bonds sheets, and is barely used.
When it fails
| Symptom | Cause | Fix |
|---|---|---|
| A sealed hollow resin part cracks days later | The trapped liquid resin never cures and pushes from inside | At least two drain holes, at opposite ends, so air can get in while the resin runs out |
| An SLS order comes back with powder inside | The cavity had no way out | Every closed void gets its drain holes |
| A standard-resin snap-fit breaks the first time you assemble it | Standard resin cannot take that strain | Print it in FDM (PETG or nylon), in SLS or in a tough resin |
| An FDM part splits along a layer | The load runs against the weak plane | Orient the part so the stress runs along the beads, or order it in SLS, which is nearly isotropic |
| A part designed for FDM is ordered in metal unchanged | A metal part carries welded supports that have to be cut and machined off, and nobody thought about where they go or how the part comes off the plate | Go over the orientation with the service before you pay |
See also
- FDM or resin for your part: the part-by-part choice between the two machines you can have at home.
- When to order the part instead: SLS, MJF, resin and metal from a service, and how to prepare the order.
- How a resin printer works: inside an MSLA machine, with its screen, FEP film and peel.
- A modern FDM printer, part by part: the machine the rest of this book focuses on.