The lid of an electronics enclosure, a board held on four standoffs, a spare part that comes with a small bag of "M3 × 8 self-tapping" screws: that is how almost every plastic appliance and most printed enclosures are held shut. A self-tapping screw needs no insert, nut or soldering iron: it forms its own thread in the plastic. Whether it holds depends on the pilot hole, the wall of the boss (the post that takes the screw), the depth and how many times you undo it. It is the cheapest anchor and the first to wear out.

How a self-tapper holds

A thread-forming screw removes no plastic. Its flanks push the wall of the pilot outwards and the plastic flows around them. That displaced plastic presses back on the wall: radial pressure in the hole and, in the boss, a hoop stress that wraps around it like a ring. That pressure is what holds the screw, through friction on the flanks and the plastic trapped between turns. Too little pressure and the screw spins freely. Too much and the boss splits open.

Thread-cutting screws have a slot in the tip and remove chips. They load the wall less, so they suit brittle materials better, but the thread they leave wears faster when you reassemble. Almost every screw sold for plastics is thread-forming.

Screws come in three families, distinguished by thread profile:

  • Screws for plastics, such as EJOT PT (30° flank) and DELTA PT (20°). The narrow flank digs deep and displaces little plastic: less radial pressure for the same grip. Plastite-type trilobular screws have a wider flank, around 48°, but their three-lobed section drags less on the way in and copes better with being undone.
  • Sheet-metal screws ST2.2, ST2.9 or ST3.5, with an ISO 1478 thread, a 60° flank and a coarse pitch: the ST2.9 has a 1.1 mm pitch against the M3's 0.5. These are the hardware-shop and consumer-electronics "self-tappers", and they work well in printed parts.
  • An ordinary machine screw, a 60° M3 with a 0.5 pitch, driven into a tight pilot. It survives only a few assemblies: its fine pitch leaves very thin plastic teeth between turns, and it is the first to strip.

In order of preference for printed parts: a screw for plastics, then sheet-metal (cheap and sold everywhere), then machine. Wood and chipboard screws behave like sheet-metal screws, with a coarse pitch and a sharp point, and work in large bosses.

M3 machine, 0.5 pitch60° flankDisplaced plasticST2.9 sheet-metal, 1.1 pitch60° flankDisplaced plasticScrew for plastics30° flankDisplaced plasticPitchPlastic between turns
At the same depth, the 30° flank displaces less plastic than the 60° one, and the coarse pitch leaves wider plastic teeth between turns. The fine machine thread is the first to strip.

The pilot diameter

The molding guide starts from pilot = 0.8 × d (its tables run from 0.7 to 0.88 × d depending on the screw). For a printed part, model the pilot at 0.8–0.85 × d: toward 0.8 in ductile plastics such as PETG, PA or PP, and toward 0.85 in stiff or brittle ones such as PLA, PC or fiber-filled grades, which do not flow around the flank: they crack.

A printed hole comes out a little smaller than a molded one, so the pilot you model is a little larger. Here d is the screw's actual outside diameter, which is why a machine screw and a sheet-metal screw with similar names do not share a row:

Modeled pilot and boss: machine screws
Screw Modeled pilot (mm) Boss diameter (mm)
M2 1.6–1.7 4
M2.5 2.0–2.1 5
M3 2.5 6
M4 3.3–3.4 8
M5 4.2 10
Modeled pilot and boss: ISO 1478 sheet-metal screws
Screw Modeled pilot (mm) Boss diameter (mm)
ST2.2 1.8–1.9 4.5
ST2.9 2.4–2.5 6
ST3.5 2.9–3.0 7
ST3.9 3.2–3.3 8
ST4.2 3.5–3.6 8.5
ST4.8 4.0–4.1 10

Molding tables give 2.4 mm for an M3; the table above gives 2.5. They do not contradict each other: 0.8 × d applies to a hole that leaves the mold at size, and a 2.5 mm printed pilot comes out closer to 2.4: a small vertical hole prints 0.1–0.3 mm tight on the diameter because of facets, the bead bulging into the curve and shrinkage (Why holes print small). That is why the table runs from 0.8 to 0.85 × d. The exact figure for your material comes from the coupon in "How to test it".

The boss: diameter and walls

The boss's outside diameter is 2 × d: 4 mm for M2, 5 for M2.5, 6 for M3, 8 for M4 and 10 for M5. With an M3, a 6 mm boss around a 2.5 mm pilot leaves (6 − 2.5) / 2 = 1.75 mm of wall per side, about 4 beads of 0.45 mm.

The reason: the forming pressure falls off with distance from the hole. With a wall of at least one screw radius, the outer face stays below the stress that would crack it. With a thinner wall, the outer face takes almost all the stress.

In the slicer, the rule is that the pilot is surrounded by at least 3 wall beads, so the thread works in solid plastic and never reaches the infill. With the 2 walls today's slicers use by default, an M3 ring comes out almost solid, but the pilot only has 2 beads of its own (0.9 mm): go up to 3 walls. In M4 and M5 the ring is wider (2.3 and 2.9 mm), and with few walls, infill ends up inside the boss: use 3 or 4 walls, or a modifier. The same applies to a pilot inside a thick wall or a block. How many walls to use is covered in Walls, perimeters and infill; the modifier, and how to handle it from the model, in Modifiers by region and height.

A free-standing boss fails at its base under a side load or overtightening, not at the thread. Tie it to the nearest wall with a rib or a gusset and round its root with a 0.5–1 mm fillet. Injection-molding rules (a boss wall at 50–60 % of the nominal wall, a draft angle) do not apply to FDM (Ribs, gussets and fillets).

Give the mouth a lead-in: a countersink or counterbore a little larger than d and 0.3 to 0.5 × d deep. The lead-in centers the screw and stops the first turn from lifting a ring of plastic or opening a crack at the top edge, where the wall has least support. On an upward-facing surface, a 45° chamfer prints without support.

dEngagement ≥ 2 × d~1 mm below the tipPilot 0.8–0.85 × dRoot filletCountersunk lead-in≥ 3 wall beadsRadial pressureScrewBoss 2 × d
The four dimensions in a section: a pilot of 0.8–0.85 × d, a boss of 2 × d, at least 2 × d of engaged thread and 1 mm clear below the tip. The thread only works in wall beads, never in the infill.

Depth: engaged thread and room below the tip

Thread engagement is at least 2 × d: 6 mm for M3, 8 for M4. In a steel nut, one d is enough. Plastic needs twice that because its shear strength is roughly ten times lower than steel's, and the plastic thread is what shears when the thread strips. Its low modulus works in your favor: the plastic gives and spreads the load across the turns better than steel on steel. Screw length = thickness of the part you are clamping + 2 × d, rounded up to the next stock length.

Make the pilot 1 mm deeper than the screw reaches, or run it through. Two reasons: the tip is tapered (long on sheet-metal screws) and does not form a full thread in its first turns, and the displaced plastic needs somewhere to go. A screw that bottoms out stops before it clamps the part, and in a blind boss it can bulge the floor.

Beyond about 2.5–3 × d, pull-out strength (the force needed to pull the screw straight out) keeps rising, but driving torque and frictional heat close in on the torque that strips the thread. From there on, change size or anchor instead of going longer.

Orientation: which way the boss splits

The usual case is an upright boss, with its axis in Z. There the hoop stress wraps around each layer along the beads, which is the strong direction. An upright boss with continuous wall loops copes well with thread forming. Its weak point is the seam, where each loop starts and ends: the crack opens there, as a vertical line up the boss. Keep the seam away from bosses: today's slicers let you paint it, place it at the back or on a face with no screws, or use a scarf seam. The options are in Where the seam goes.

A boss lying on its side, with a horizontal axis, is the opposite case. The hoop stress crosses the layers and the boss splits along a layer line with much less force. If a pilot has to be horizontal, take the boss up to 2.5–3 × d in diameter or switch to an insert. A pilot of 6 mm or less does not need a teardrop shape: it comes out round enough.

Pull-out depends on orientation too. Upright, a stripped thread shears along a vertical cylinder that cuts through every layer, so layer adhesion plays no part in it. What loads the Z direction is the boss as a whole: pulling on the screw tears it off along a layer line, almost always at the root or in the first layers above the base. Assume Z holds half of what XY does, and only 30 % in fiber-filled materials (Layer adhesion and anisotropy). Lying down, the surface the thread shears along runs partly along the interfaces between layers, and there adhesion governs. That is why a self-tapped boss is fine for a lid and not for hanging a weight.

Upright bossStress along the beadsSeamCrack at the seamPull-out loads the boss in ZZBoss on its sideCrack along a layer lineStress across the layersZ
Upright, the hoop stress runs along the beads and the crack appears at the seam; lying down, it crosses the layers and the boss splits along a layer line. Pulled on, an upright boss tears off along a layer near the root.

Material, tightening and reassembly

  • PLA grips well but is brittle: pilot at the high end. It also creeps: it loses its clamping force within weeks, sooner with heat. Under a sustained load, PLA is only comfortable below about 30 °C and its limit under load is around 40 °C, so a PLA enclosure in a car in the sun or next to a motor works loose. The plastic clamped under the head flows too: a wide washer or a flanged head spreads the pressure and delays loosening. The mechanism is in Creep and fatigue.
  • PETG takes a tighter pilot and cracks less.
  • ABS and ASA are the classic materials for molded bosses and take self-tappers very well.
  • PA holds a screw best because it is tough, but it absorbs moisture and swells.
  • Fiber-filled: pilot at the high end, brittle walls.
  • TPU: unsuitable; it yields and the screw cannot grip.
  • Resin: standard resin is so brittle that a self-tapper almost always cracks it; use an insert or a nut. Only tough resins take a self-tapper, with the pilot at the high end.

Tighten by hand or with a slow driver and the clutch set low, never with an impact driver. The first drive forms the thread and needs the most torque: stop as soon as the head seats. In plastic, the margin between the head seating and the thread stripping is tiny, and friction at high speed softens PLA. Do not lubricate with oil: it lowers friction, so the same turn clamps far harder and strips the thread or splits the boss, and some oils crack ABS and PC. For the same chemical reason, avoid anaerobic threadlockers on ABS and PC.

A thread-forming screw survives about 10 assemblies if it goes back into its own thread. To get it there, turn it backwards with light pressure until you feel the click of the thread dropping into its groove, then tighten. If you drive it straight in, it cuts a new thread across the old one and the boss strips within a few cycles. Screws for plastics cope better with reassembly. If you expect more than 10 cycles, fit an insert or a captive nut from the start.

When it fails

Symptom, cause and fix
Symptom Cause Fix
The screw turns but never tightens Pilot too large, short engagement, or a machine-screw pilot with a sheet-metal screw Pilot 0.1 mm smaller, a deeper hole or the next size up
The boss splits lengthwise as you drive the screw Pilot too tight or wall too thin Larger pilot, thicker boss, move the seam away
It needs a lot of torque, squeals or smokes and the thread comes out melted Too much speed or a tight pilot; friction softens PLA at around 60 °C Slow down, use a hand screwdriver
The mouth bulges or lifts a ring of plastic No lead-in Add the countersink or the chamfer
The thread strips after a few assemblies Screw driven straight in every time Turn backwards to the click before tightening
The boss snaps at the base Free-standing boss, no fillet Rib to the wall and a 0.5–1 mm fillet
The enclosure works loose over the weeks PLA creep, worse with heat Wide washer, another material or an insert

If the thread has already stripped, try these in order. First, the next size up or a longer screw, if the boss has room for it. Next, a drop of thin cyanoacrylate in the hole; let it cure and drive the screw again: it gives the hole a second life. Last, open the hole out to the insert size (4.0 mm for an M3) and fit a heat-set insert. An M3's 6 mm boss leaves only 1 mm of wall around a 4.0 mm hole, below the 1.6 mm the insert needs. If you think you will end up with an insert, size the boss for it from the start: 4.0 + 2 × 1.6 = 7.2 mm at least; draw it at 8 (Designing for heat-set inserts).

How to test it

To tune the pilot, print a coupon: for an M3, three pilots of 2.4, 2.5 and 2.6 mm in your material, and test them with the screw you will actually use. Keep the tightest one that goes in by hand without leaving a whitish stress line or a crack at the mouth. When in doubt, err on the large side. A loose pilot loses a little grip; a tight one splits the boss. How to design the coupon is in Test coupons.

There is no pull-out force or tightening torque you can copy from a table for a printed part: they depend on the material, the profile and the orientation. If the joint carries load, print the boss exactly as it will sit in the part and test it.

See also

Design it in KapyCAD

Draw the part with these clearances and walls, and change any dimension later without redrawing it.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?