You print a rain gauge cup in PETG, fill it to the brim and leave it on the shelf. In the morning there is a damp ring on the shelf and a vertical row of droplets down one side. No cracks. The water has found the gaps between the beads and wicked along them by capillary action, pushed by nothing more than a few centimeters of head (≈ 1 kPa per 10 cm). What seals it is mostly the number of walls, the flow and where the seam sits; a coating only patches what is left.

Where the water gets out

Water does not pass through the plastic. It travels along the continuous channels between beads, and capillary action helps it along even when almost nothing is pushing.

WaterWet sideBedWall-floor junctionGaps between wallsPinholeWallFloorSeamSealed wall
Water escapes through channels between beads: the wall-to-floor junction, the gaps between walls, a missing bead and the seam stacked layer on layer. More walls, more flow and a rounded corner close them.

Prusa measured this with cylindrical test pieces and with submerged parts (Prusa blog, "Watertight 3D printing", parts 1 and 2, from here on "the trial"; Prusa calls walls perimeters). The leaks came mostly through the seams and through the transition between the walls and the solid infill, not through the bond between layers. Untreated PETG leaked almost at once, at the low pressure of a bucket, and exactly at those spots. There are four paths, from most to least important:

  1. The Z seam. Every layer starts and closes its loop in the same place. The start comes out thin and the end fat, so an aligned seam adds one slit per layer until it opens a vertical channel. The mechanism is in Where the seam goes.
  2. The junction between wall and solid infill. Where the solid infill of the floor or the lid meets the inner wall, it leaves an annular slit. Inside a cup, that is the corner between floor and wall.
  3. The gaps between walls. Round beads leave diamond-shaped gaps between them. With enough flow and overlap they close; with under-extrusion they link up into channels. If the thickness is not a whole number of walls, the slicer fills the remainder with gap fill, which leaves even more.
  4. Pinholes. A bead that breaks for an instant, from a partial clog, bubbles from wet filament or a dirty nozzle, leaves a hole straight through a thin wall. In the trial, wet PETG bubbled: dry the filament and print with a clean nozzle.

That is why 100 % infill alone does not make a part watertight, and why a thin wall with sparse infill behind it is worse: its cells fill with water.

Design a wall the slicer can close

Draw the thickness as a whole number of walls, not as a round figure in millimeters. With a 0.4 mm nozzle the slicer overlaps the 0.45 mm wide beads and spaces the walls about 0.41 mm apart, so n walls take about n × 0.41 + 0.04 mm: 4 walls are about 1.7 mm and 6 about 2.5 mm. At that thickness the slicer fills the wall entirely with walls, with no infill; check in the preview that no gap fill appears. The trial starts from 4–6 walls. Outside spiral mode, with a 0.4 mm nozzle, a two-line wall measures 0.9 mm and is the minimum; a functional part gets three lines, 1.2 mm. Every wall and infill setting is covered in Walls, perimeters and infill.

Material only matters in thin walls. In the trial's cylinders, the minimum number of walls that held water was:

Minimum walls to hold water (Prusa, blog “Watertight 3D printing pt. 1”)
Walls Materials
2 ABS, ASA, CPE, PC, PP
3 TPEE
4 PETG, PLA, PA
5 HIPS, PVB

With 6 walls (about 2.5 mm), the material stopped mattering. That is one lab's result, with one printer, 0.15 mm layers and machines and filaments that are now years old. Read it as a ranking, not a guarantee.

Keep the thickness constant across the wall. A boss, a raised label or a fill-level mark deflects the walls and adds starts and stops; the trial lists bosses among the causes of leaks. Engrave labels on the outside, less than one bead deep, or move them to another part.

Round the inside corners. The sharp corner between wall and floor is where the leak ring sits and, under pressure, where the bending concentrates (more on that below). Give it an inside fillet with a radius equal to or greater than the wall thickness, with "Ensure vertical shell thickness" turned on: the near-horizontal part of the fillet prints in steps with solid infill, and every step is another junction. A 45° inside chamfer prints with walls only and avoids the problem.

Every hole in a wet wall adds a seam and a junction. Bring cables and tubes out through the lid, not the wall. For screws, use blind bosses and heat-set inserts that stop short of the wet side; the insert pocket is designed in Designing for heat-set inserts.

The settings that close the wall

Before you touch any setting, calibrate the flow (Extrusion problems): adding 5 % to a badly calibrated flow tells you nothing. With the flow calibrated, these are the starting values for a watertight part with a 0.4 mm nozzle:

Settings for a watertight wall (Prusa Knowledge Base “Watertight prints” and blog pt. 1)
Setting Value for watertightness Why What it costs
Walls 4–6 Each extra wall is another barrier and moves the seam and the junction away from the wet face Time and plastic
Flow +5–10 % over the calibrated value, or line width +5–10 % (0.40 → 0.44 mm) The extra plastic fills the diamonds between beads Larger dimensions, rougher faces, more stringing in PETG
Temperature +5–10 °C, up to the top of the filament's range Hot beads flow over each other and weld better More stringing and worse bridges
Layer height 0.15 mm; never more than 60–65 % of the nozzle diameter More overlap per layer, smaller gaps Print time
Bottom and top layers ≥ 5 Margin in floor and lid Little
Solid infill to wall overlap 25–35 % if the floor weeps at the edge Closes the annular slit at the wall-floor junction A slight bulge at the edge

The trial tested layer heights from 0.05 to 0.30 mm: 0.05 sealed best and 0.30 worst. In the floor, with 8 walls, any number of bottom layers between 2 and 7 sealed: they count for less than walls, and 5 is a safe value. Why heat welds better: Layer adhesion and anisotropy.

Setting names and defaults change between versions. As of late 2026, PrusaSlicer calls the overlap "Infill/perimeters overlap" and Prusa gives 10 % as its starting value; in OrcaSlicer and Bambu Studio it is "Top/bottom solid infill/wall overlap", with a default that varies by profile, so check yours before raising it. Leave "Ensure vertical shell thickness" on (in OrcaSlicer, "All" by default): it keeps the shell thickness on sloping walls.

Align the seam or paint it somewhere you can see and seal: a corner or the back face. If your slicer offers a scarf seam, turn it on: it ramps the start and end of each loop over each other (Where the seam goes). A random seam spreads weak points over the whole wall; avoid it on a wet part.

Dry the filament (Drying and storing filament). Wet PETG or nylon bubbles, and every bubble is a pinhole.

Spiral (vase) mode prints a single wall, with no seam and no junction with the infill. In the trial it held water in every material tried. But that wall is about 0.45 mm with a 0.4 mm nozzle: it is fragile and any under-extrusion opens it. Fine for a decorative vase; not for something handled or pressurized. Advanced toolpaths explains how it works, and also height-staggered walls (brick layers). Some users report that brick layers seal better; no reliable data confirms it.

Orientation and pressure: where a vessel opens

Print containers upright, mouth up. The floor sits on the bed, and its first layer, squashed against the bed, is the tightest face the printer can make (The face on the bed). The wall's layers end up as horizontal rings.

Opens herePressure pσz = p·r/(2t)Across the layersσθ = p·r/tAlong the beadsPressure pEdge momentFlat endFillet r ≥ tDomed end
Under internal pressure, hoop stress runs along the beads and axial stress, half as large, crosses the layers. The wall opens at the vertical seam. The weak point is the flat end and its corner: it calls for a thicker floor and wall base, with a fillet, or a domed end.

In a thin-walled cylinder with internal pressure p, radius r and wall thickness t:

  • hoop stress σθ = p·r/t, running round the cylinder within each layer, along the beads;
  • axial stress σz = p·r/(2t), along the axis, across the layers.

The weakest direction, the one across the layers, carries exactly half the stress. For design, assume the part is half as strong in Z as in XY, or 30 % if the material is fiber-filled (Layer adhesion and anisotropy).

That decides where it opens. A vertical-axis cylinder under internal pressure does not split between layers: it opens at the vertical seam, the one line where every layer is cut. Put the seam where it does no harm and give it walls to spare. Lying down, the same cylinder loads its sides with hoop stress across the layers and splits along one of them. Never print a pressurized tube lying down.

The weak point of a printed vessel is its flat end and the corner where it meets the wall, not the wall. In a circular plate clamped at the edge under uniform pressure, the maximum stress is at the edge: σmax = 0.75·p·r²/t² (Roark, Formulas for Stress and Strain, flat plates, fixed edge). The moment at that edge, M = p·r²/8 per millimeter of perimeter, bends the base of the wall across its layers. And the wall is not a perfect clamp: it rotates a little, the edge moment drops and the center of the floor works harder. If the edge rotated freely (simple support), the center would reach σ = 1.24·p·r²/t². Size the floor with the supported case and the wall base with the clamped moment.

An outward-domed end works as a spherical cap, σ = p·R/(2t), with R the radius of the cap's sphere. Only a hemispherical end has R = r and matches the axial stress; the flatter the cap, the larger R and the stress, and its joint with the wall, which the cap pulls inwards, needs reinforcing. Printed upright, it also does not sit on the bed, and it starts as a near-horizontal overhang. Give it a printed support ring that reaches the bed, keep the overhang to 45° or less, or print it separately and glue it on. An inward-domed end works in compression and can snap through.

Pressure pushes the lid with F = p·A, and that force sizes the screws or the thread of the closure (O-ring grooves, Enclosure lids). A is the area out to the seal line: the inside diameter if the O-ring seals radially, the O-ring diameter if it seals on the face.

With external pressure, as on a submerged housing, add a little under 1 bar per 10 m of water: at 20 m, about 2 bar. A wall that held in a bucket can weep at depth. If the wall is thick enough to have infill, the trial suggests 4 walls and 60 % infill as a starting point; its part with 3 walls and 15 % infill held at 1 m, with the warning that it may fail at 30 m. Buckling of thin walls under external pressure is not covered here.

Worked example: a canister at 2 bar

A closed cylindrical PETG canister, Ø50 mm inside (r = 25 mm), printed upright, flat floor on the bed, O-ring lid, p = 0.2 MPa (2 bar).

Allowable stresses. The PETG Basic datasheet gives 51 MPa in XY and 35 MPa in Z; for design, take 50 % of XY in Z: 25.5 MPa. Because the load is sustained and a failure can hurt someone, use a safety factor of 4 (Estimating whether a part will hold, Creep and fatigue). Along the beads: 51 / 4 ≈ 12.8 MPa. Across the layers: 25.5 / 4 ≈ 6.4 MPa.

Wall for strength.

  • Hoop, along the beads: t ≥ p·r/σ = 0.2 · 25 / 12.8 ≈ 0.39 mm.
  • Axial, across the layers: t ≥ p·r/(2σ) = 0.2 · 25 / (2 · 6.4) ≈ 0.39 mm.

Strength asks for less than one bead.

Wall for watertightness. PETG needed 4 walls in a thin wall (about 1.7 mm), and untreated it let water through even in a bucket. At 2 bar in PETG you need both: at least 6 walls (≈ 2.5 mm) and a coat of epoxy inside.

Flat floor. With a supported edge, the worst case for the center: t ≥ √(1.24·p·r²/σ) = √(1.24 · 0.2 · 625 / 12.8) ≈ 3.5 mm. The stress at the center lies in the plane of the layer, along the beads.

Wall base. The edge moment, M = p·r²/8 = 0.2 · 625 / 8 ≈ 15.6 N·mm per mm, bends it across the layers, with σ = 6·M/t² and 6.4 MPa allowable: t ≥ √(6 · 15.6 / 6.4) ≈ 3.8 mm. With the 2.5 mm wall, that base would work at about 15 MPa, more than twice the allowable. The fix: a floor of about 4 mm and the first few millimeters of wall at 10 walls (about 4.2 mm with 0.15 mm layers), joined with an inside fillet or chamfer; or a domed end with its support ring and a reinforced joint.

Lid. If the O-ring seals radially, against the inside diameter: F = p·π·r² = 0.2 · π · 625 ≈ 390 N. If it seals on the face, at a diameter of about 58 mm: F ≈ 0.2 · π · 29² ≈ 530 N, as if 53 kg were pushing the lid outwards. Size for the larger figure. A single clip will not do: you need a thread or 4–6 screws, worked out in O-ring grooves and Enclosure lids.

Settings. 6 walls, flow +5 %, 0.15 mm layers, 5 bottom layers, nozzle temperature at the top of the PETG range, seam aligned on the back face and dry filament. Before you trust it, run the water pressure test from "How to test it" at 1.5 × p, that is, 3 bar: that is common practice in hydrostatic testing, not a standard.

Sealing after printing

Fix the print first; coat afterwards. A coating closes isolated pinholes; it does not rescue a porous print. Coat the face that touches the water. Technique, cure times and film thickness are in Coatings and epoxy; this section only helps you choose.

  • Low-viscosity epoxy on the wet side. In the trial, PETG with epoxy did not leak at depth. It works well, but it is messy and slow to cure.
  • Thin cyanoacrylate, which wicks in by capillary action, for a seam or a small part.
  • Acrylic spray lacquer, several coats inside and out, for undemanding parts.
  • Vapor smoothing, only on ABS, ASA, PVB or HIPS, and it seals only the outer surface: the trial's smoothed ASA still let water through, slowly, at depth (Vapor and chemical smoothing).

A rigid coating cracks on a part that flexes: TPU, a thin working wall, a bellows (Accordion bellows). There, the print has to provide the seal. In the trial, epoxy cracked under pressure on walls 1–2 beads thick: coat only walls that are already stiff, 4 beads or more.

Mask mating surfaces and O-ring grooves with tape: the film changes their dimensions.

Watertight does not mean food-safe (Printing for food contact).

Hot water and material

In hot water, PLA softens near its heat deflection temperature (57 °C at 0.45 MPa). Under a sustained load, PLA is only comfortable below about 30 °C and its limit under load is around 40 °C; PETG's is around 50 °C (Creep and fatigue). For hotter liquids, use ASA (up to about 80 °C under load), PC (about 95 °C) or unloaded PP. In the trial, PLA did not dissolve; over months of immersion it may absorb water and swell slightly, but that was not measured.

When it fails

When it still weeps: symptom, cause and fix
Symptom Cause Fix
Vertical line of droplets or a damp stripe Aligned seam letting water through Move the seam to a corner or the back face, scarf seam, flow +5 %, seal that line with thin cyanoacrylate or epoxy
Damp ring at the base with a dry wall Wall-floor junction More solid infill to wall overlap, more walls, inside fillet or chamfer, coat the inside corner
The whole wall slowly "sweats" Too few walls or under-extrusion Calibrate the flow, then 4–6 walls, thinner layers, higher temperature
One or two pinholes Bubble from wet filament or a partial clog Dry the filament, clean the nozzle (Extrusion problems), seal the spot
Holds in the bucket but weeps under pressure or at depth Wall too thin, or sparse infill behind too few walls A wall made entirely of walls; if it is thick enough to have infill, 4 walls and 60 % as a starting point; epoxy inside; check the flat end and its corner
Weeps only around a screw, a label or a cable or tube pass-through Deflected walls or a through-hole Blind boss, move the feature to the lid, uniform wall thickness
Was watertight at first and weeps after weeks of use Coating cracked by flexing, or PLA softened by hot water Stiffer wall under the coating, material with a higher service temperature

How to test it

Before you start a six-hour vessel, print a test coupon: a small cup with the same settings (Test coupons).

Paper test. The basic test, with no pressure. Fill the part and leave it upright for 24 h on dry kitchen paper. A stain is a leak path.

Dyed water. A few drops of food coloring in the water mark the path: a line at the seam, a ring at the base or a dot at a pinhole. Each pattern has its fix in the "When it fails" table.

Printed cup holding blue water: droplets in a vertical line over the seam and a blue ring on the paper around the base; the rest of the wall dry
Printed cup holding blue water: droplets in a vertical line over the seam and a blue ring on the paper around the base; the rest of the wall dry

Bubbles. More sensitive, and it works for sealed enclosures too. Pump air in at a few hundred mbar with a syringe or a rubber bulb through a barb (Hose barbs and fittings), with the part submerged or brushed with soapy water. If the bubbles come from the closure line, the problem is the seal; if they come from the wall, the problem is the wall.

Water pressure test. For a part that will work under pressure: fill it completely with water, with no trapped air, raise it to 1.5 times the working pressure, hold for 10–15 minutes (common practice, not a standard) and inspect. Water, being almost incompressible, stores hardly any energy; air does. Every test at 1.5 × p adds creep to the plastic: do it once per part, never repeatedly on the same one.

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?