kapy academy

Testing a mechanism before you trust it

18 min readUpdated Nov 2026

A box with two snaps in the lid clicks shut ten times in a row on the desk and, a month later, pops open inside a backpack: the snaps have relaxed. Testing it by hand only checked the first cycle, at 20 °C. Before you trust a mechanism, ask it three questions, each with its own test: does it give the force you designed it for (the force-travel curve), does it survive the cycles of its life (the cycle rig), and does it keep its force and shape over time and heat (the 48-hour test).

Set the pass mark before you print

A test without a number to beat ends in "seems fine". Before you print, write down three numbers: the force window, the life in cycles and the service temperature.

The force window has two edges. The lower one is what you need to hold; the upper one is the most a hand will apply without a struggle. The holding force comes from what the part has to hold: the weight times a margin for accelerations. A phone mount in a car calls for (F + W) / W ≥ 3, where F is the holding force and W the weight of the phone, as Phone mounts explains. Do not take the actuation force from an ergonomics table: find a product you like the feel of and measure it with the same instrument you are going to use.

Count cycles as in Creep and fatigue. A snap opened twice a day for five years adds up to about 3,650 cycles. A hinge opened ten times a day reaches 18,250 over the same period.

Under load, an unfilled part works up to about 15–20 °C below its HDT at 0.45 MPa: PLA about 40 °C, PETG 50, ABS 70, ASA 80, PC 95 (Heat, cold, sunlight and chemicals). If the part will run close to that ceiling, run the 48-hour test hot.

You need at least two parts printed with the same settings and the same orientation: one alone is an anecdote (Estimating whether a part will hold). And the part you test is the one you will actually print: final material, profile, orientation and seam position. A coupon in another orientation is a different part (Layer orientation for mechanisms).

The force-travel curve

One number is not enough: the curve carries several. The peak while pushing is the insertion force. The sudden drop is the click you feel. The negative stretch on the way out is the retention. The area of the loop between the outward and return paths is lost energy: the jump at the click, friction and the plastic's own damping. In a spring with no click, nearly all of it is friction. Each mechanism has its own signature curve: a detent gives a torque peak per notch, a bistable passes through zero force, and a spring gives a straight line whose slope you compare with the stiffness worked out in Leaf and cantilever springs or Coil springs.

TravelForcepushpull0insertion forceclickretention forcelost energy (hysteresis)freshly printedafter cycles or 48 h
The insertion peak is what it takes to close; the negative peak on the way out is what holds. The loop area is energy lost in the click and in friction. The dashed curve is the same snap after relaxing: it holds less.

What to measure with

Instruments for measuring force at home (indicative values)
Instrument Resolution Good for Watch out for
Kitchen scale used as a load cell 1 g = 0.01 N slow stepped curves: part on top, you push down fast peaks; auto-zero
Digital push-pull force gauge with peak hold 0.1 N; accuracy ±0.5–1 % of full scale the only one that catches the peak of a fast click full scale: for snaps, 10–50 N
Load cell + HX711 amplifier + microcontroller steps of hundredths of a newton logging a whole curve zero drift with temperature; at 10 samples/s it misses the peak; switch it to 80

Do not confuse resolution with accuracy. A force gauge's accuracy is a percentage of full scale, not of the reading: on a 500 N gauge, ±0.5 % is ±2.5 N, more than the whole band in the example below. A cheap load cell shows hundredths and still its zero moves with temperature and with how it is mounted; badly mounted, it can be out by several percent. Zero it every session and calibrate it with a known weight. Many kitchen scales, and some luggage scales, come with automatic zero tracking and auto power-off: they pull a slowly changing load back to zero, and a stepped curve is exactly that. Turn it off if you can, or check with a known weight that the reading does not wander on its own over 2–3 minutes.

Fix the travel, read the force

A repeatable curve comes from moving the part in fixed steps and reading the force at each one, not from pushing by hand and watching the display. The cheapest rig is a printed bridge with an M6 screw (1 mm pitch) pushing on the part, which sits on a kitchen scale. One turn is 1 mm; a quarter turn, 0.25 mm. Read the scale at each step, out and back. The bridge's feet rest on the table, off the scale, so their weight stays out of the reading. The screw tip must not turn against the part: push through a guided plunger or a ball tip, or the rotation adds friction and torsion to the reading.

To read the return stroke, where the snap pulls upwards, the base has to be fixed to the platform with double-sided tape or a cable tie, the plunger has to be attached to the moving half (a captive nut in it does the job) and the scale has to show negative values after taring with everything mounted. Not all of them do: check before you start. Pulling by hand with a luggage scale only gives you the peak, and only if you pull slowly.

Three front panels. On the left, the force rig: an M6 screw in a printed bridge that stands on the table, off the scale, lowers a carriage with the example's PETG clip until it snaps into its box on the scale, then pulls it back out. In the middle, what the scale reads against the travel: a dot rides the push curve, with the 2.7 N insertion peak and the click, and the pull curve, with the 5.3 N retention peak below zero. On the right, the cycle rig: a gear motor turns a crank of radius r whose rod drives a pusher down a guide; its collar lands on the fixed stop at the end of each 2r stroke while it presses a cantilever key.
On the left, the screw fixes the travel and the scale reads the force. On the right, the crank repeats the real travel and the stop keeps it from going past. In the middle, the scale's reading over one cycle: the curve comes from the ramp formula with μ 0.4, and the arms are drawn rigid, pivoting 0.15·L from the root.

Four rules for a reading you can trust:

  • Push along the real actuation axis, with a guide: pull 20° off-axis and you read only cos 20° ≈ 0.94 of the force (6 % low), and you bend the part as well.
  • Zero the instrument with the fixture already mounted.
  • Repeat five times and keep the worst case on each side: the lowest retention and the highest actuation force, like the five pulls in Phone mounts.
  • Note the room temperature.

Worked example: predict, then measure

A PETG cantilever snap for the box lid: arm L = 15 mm, thickness t = 1.5 mm, width w = 6 mm, catch height y = 1.0 mm, a 30° lead-in ramp and a 45° retention face, both angles measured from the insertion axis. The formulas come from Print-friendly snap fits; this section only applies them.

  • Strain: ε ≈ 1.5 · t · y / L² = 1.5 · 1.5 · 1.0 / 225 = 1.0 %. That is under the 2 % PETG tolerates in repeated use.
  • Arm force: P = w · E · t² · ε / (6 L). With E = 1.6 GPa, the design modulus of PETG, P ≈ 2.4 N.
  • Force at the ramp: F = P · (tan θ + μ) / (1 − μ · tan θ), with μ = 0.3–0.5 for printed plastic on printed plastic: friction between plastics is a range, so work with both ends (Friction and wear). Closing, at 30°: 2.5–3.6 N. Opening, at 45°: 4.5–7.2 N.

The uncertainty in friction alone is enough to swing the retention by 60 %, from 4.5 to 7.2 N: that is why you measure it.

Mount the snap in the screw rig, push until it engages, then pull until it comes out. Read both peaks, insertion and retention, and compare them with the two bands. A reading below the band points to an arm thinner than planned or a lower catch: measure both with callipers. Above it, to a thicker arm or a rough ramp. Fix the geometry in the parameter, not with sandpaper.

The home-made cycle rig

By hand, with a tally counter, you get to a few hundred cycles: the 20 openings that articles such as 35 mm DIN rail ask for, or the 50 that Clickfinity and CLICKbase suggests. Beyond that you need a machine. Three rigs, from cheapest to most elaborate:

  1. A hobby servo driven by a microcontroller board, working the part (the button, the lever) through a short link. The program itself counts the cycles.
  2. A 12 V DC gear motor at 30–60 rpm turning a crank or an eccentric. The stroke is twice the crank radius (Crank-sliders and eccentrics). A microswitch, or a magnet on the crank and a reed switch, sends the pulses to the counter.
  3. For lids and hinges, a cam that lifts the lid and lets it drop (Cams and followers).

You can print the rig too, but its frame has to be much stiffer than the part; otherwise you are measuring how much the rig bends.

Copy the real travel, overtravel included. Users push all the way to the end stop, so the rig has a fixed stop and the crank never drags the part beyond it. Work the mechanism the way a finger would: do not bend the flexure sideways.

Run at 0.5–1 Hz. The plastic self-heats on every cycle through hysteresis (Creep and fatigue), and a fast rig breaks a part a hand never would. After the first few hundred cycles, measure the temperature at the root of the arm: an infrared thermometer at 1–2 cm, because any further away the spot it reads is wider than the root, or a fine thermocouple taped to it. If it is several degrees above ambient, slow down. At 1 Hz you get 3,600 cycles an hour: the snap's 3,650 in a little over an hour and the hinge's 18,250 in about five.

How many cycles? At minimum, the life you wrote down; better, two to three times that life, on two parts. Plastic has no reliable fatigue limit and the scatter between printed parts is large.

You do not need to measure all the time: measure the force curve and the play at 0, 10, 100, 1,000 and 10,000 cycles, one point per decade. Over the first 10–100 cycles the force usually drops a little as burrs and layer ridges wear down. That is running-in, not a failure: take the value after running-in as your starting value (Friction and wear). Measure the play as Clearances for moving parts explains.

Before you start, write down what will stop the test: a crack or stress whitening at the root, the force outside the window, more play than the mechanism tolerates, or a new noise. Whitening at the root announces the fatigue crack: stop, take a photo and note the cycle count.

A rig that runs all night is an unattended machine: a low-voltage motor with its own supply, fingers away from the crank and nothing flammable underneath.

The 48-hour test

Creep shows up in two ways, and each is measured differently (Creep and fatigue). Under constant load (a hook, a hanger, a device on a bracket) the deflection grows. Under constant displacement (an engaged snap, a clip on a tube, a press fit, a preloaded detent, a screw in plastic) the force drops: that is stress relaxation.

Under constant load, hang the real weight, or water bottles of the same weight at the same distance. Mark the position of the edge with a pencil line on the wall or measure it with a dial indicator. Check it at 1 h, 24 h and 48 h; for anything that hangs on a wall, also at 7 days, as VESA: the 75, 100 and 200 patterns recommends.

Under constant displacement, each reading uses up a specimen: opening a snap restarts its relaxation. Engage one part per reading (three for 1 h, 24 h and 48 h, six if you do them in duplicate) and, before engaging them for the test, measure each one's retention on day 0, after running-in. When a part is due, open it and measure with the same instrument and the same method. Record each reading as a fraction of its own starting value: that removes the scatter between parts. Also keep a twin from the same print unengaged, and measure it at the end: it separates relaxation from what aging and moisture change. It is the same idea as comparing against an empty cell in Clickfinity and CLICKbase.

Why 48 hours? Primary creep is fast and then slows down. The span from 1 h to 48 h is 1.7 decades on a logarithmic time scale, and on that scale the loss per decade is almost constant (Creep and fatigue). Three readings are enough to see the trend and extend it; a fourth at one week confirms it and shortens the extrapolated stretch. The result is not a measured life: it is a straight line through a few points, extrapolated, at the test temperature.

time, log scaleretention force1 h1 day48 h1 week1 month1 yearforce each snap needsunengaged twin partmeasuredextrapolatedmargin
On a logarithmic time scale the loss is almost a straight line: three readings in 48 h give the trend, one at a week confirms it, and extending it tells you whether it is still above what the lid needs after a year.

Worked example: extrapolating

These readings are made up to show the arithmetic; they are not PETG data. The snap retains 5.6 N at one hour and 5.1 N at 24 h. The two are log₁₀ 24 ≈ 1.38 decades apart, so it loses about 0.36 N per decade. At 48 h (1.68 decades) the line predicts 5.0 N: check it against the third reading. If it agrees, the line holds. A year is 8,760 h, 3.94 decades after the first hour: 5.6 − 0.36 · 3.94 ≈ 4.2 N.

If each of the two snaps has to give 4 N for the lid to stay shut with some margin, this one is cutting it fine. The fix is in the design: an arm that sits straight, undeflected, once engaged; a material that creeps less (Which plastic for which mechanism); or a positive lock. A deeper catch does not fix it: more strain relaxes faster or whitens the root.

Hot

If the part will run hot (in the car, by a window, near electronics), run the 48 hours at that temperature. If you do not know it, run the hot test at the service temperature under load: 40 °C for PLA and 50 °C for PETG. A filament dryer holds 45–70 °C on a thermostat (check that its timer reaches 48 h, or restart it when it runs out); a closed printer enclosure works too. Always put a thermometer next to the part. Keep the service ceiling under load in mind: above it creep speeds up sharply, and near the HDT the part gives way in hours. Never run a hot test in the kitchen oven unattended.

Three traps that skew the test

When you remove the load, wait 24 h and measure again: what does not come back is permanent set (Creep and fatigue). Measure straight away and you count as permanent what was still recovering.

Do not use a cheap load cell to measure for 48 hours straight. Its zero drift can be of the same order as the relaxation you are looking for. Use dead weights and a position mark, or unload it and check the zero before each reading.

A freshly printed part creeps a little more than one a few weeks old, because of physical aging. Testing a fresh one keeps you on the safe side; what you cannot do is compare a fresh part with its rival from a month ago.

Shake it and pull it

Two kinds of abuse slip past both the rig and the 48 hours. Shake the part hard, with the real device fitted: you should feel no play and hear nothing rattling in its seat. Then pull five times in the worst direction and keep the lowest value. If the mount will carry a device outdoors, tie it on with a safety lanyard for the first few outings, as Garmin-compatible quarter-turn mounts advises. Repeat the shake after the hot 48 hours. A seat that was tight when cold can come out loose, as Watch straps and lugs warns.

Write down what you tested

Write one line per part (date, material and color, printer and profile, orientation, parameter, cycles, forces with the instrument used, temperature and verdict), change one thing per batch (Iterate and measure) and keep the tested parts, labeled: they are where the next design starts.

When it fails

Symptom → cause → fix
Symptom Cause Fix
Force drops over the first 10–100 cycles, then holds Running-in of ridges and burrs Take the starting value after running-in; it is not a failure
Cracks on the rig much sooner than by hand Overtravel past the real stop, or self-heating from a high rate Fixed stop on the rig, 0.5–1 Hz, root temperature measured up close
Snaps cleanly along a layer at the root, with hardly any whitening Arm printed standing up: the bending crosses the layers Arm length in the layer plane (Layer orientation for mechanisms)
Passes on the rig, fails in use Heat, users pushing past the stop, or the final part changes orientation, material or seam Hot 48 h, test the final print, stop built into the part itself
Readings swing ±20 % between repeats Off-axis pull, luggage scale swinging, missed peak, scale auto-zero Guide, slow pull, peak-hold force gauge, worst of five
Load cell reading drifts overnight with nothing changing Zero drift of the cell itself and its mounting Dead weights and a pencil line; unload and check zero at each reading
Whitening at the root after a few thousand cycles Strain above the repeated-use limit, or a sharp root Longer or thinner arm, root fillet r ≈ 0.5 t, a material that takes more strain (limits in Print-friendly snap fits)
Play keeps growing with cycles Wear on a pin or a guide Friction and wear
Holds on day one; weeks later the lid pops open Relaxation of an arm left deflected when engaged Straight arm once engaged, positive lock, a material that creeps less

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?