You print a PLA turntable in place and it comes off the bed rattling, with 0.8 mm of axial play. Every horizontal gap had to be one layer plus 0.2 mm of air, and the ceiling over it sagged anyway. Print the same turntable with two thin PETG rings in those gaps and it turns quietly, with flat faces. Inside a joint, the second material touches without bonding, dissolves, or is the part that bends, and it pays off in the horizontal gaps, the ones that cost play and finish.

Where the second material goes

Start from the single-material figures: a print-in-place part needs about 0.3 mm of gap per face in PLA (0.25–0.4 on a modern machine) and, in Z, at least one layer plus 0.2 mm of air, rounded up to whole layers: 0.4 mm with 0.20 mm layers (Print-in-place clearances). The ceiling over that horizontal gap is a bridge that sags into it. The vertical gap is cheap and reliable; the horizontal one costs you play and surface finish.

Hence the rule: put the second material in the horizontal gaps and leave air in the vertical ones. The horizontal ones are the thrust faces, the ceilings and the captive heads. On a horizontal face, the second material replaces "layer + air + sagging ceiling" with one printed layer that the face above rests on flat. On a vertical face, air already works at 0.3 mm, and you cannot fill that gap with another material: the second material has to be at least one bead wide (about 0.35–0.4 mm with a 0.4 nozzle) or the slicer drops it. If you want it there, it takes up part of the wall. Step through the preview layer by layer and check that the second material is actually there.

The exception is zero radial play: a bushing that must not vibrate, gear teeth without backlash. There a sleeve or tooth flank of the non-bonding material on the vertical faces is worth it, even though it costs you material changes. Gears are covered in Print-in-place gearbox.

layer + 0.2Sagging ceilingBaseLidPivot0.3Axial playOne materialTrapped washer0.3Non-bonding pairOne layerWater0.3Axial playSoluble
The same captive turntable in three versions. The second material replaces the horizontal gaps and their sagging ceilings; the pivot hole keeps its air gap.

Non-bonding pair: the gap, filled

PLA and PETG touch without fusing. That is why each works as a support interface for the other, as Prusa documents for the XL; which other pairs bond and why is in Functional multi-material parts. In a joint, that interface is printed in contact, with no air modeled in Z, and the face above comes out flat, as it does over a support interface with a Z distance of 0 (Support materials).

A layer of PETG between two PLA bodies bonds to neither, so once printed it is a loose part. Either the geometry traps it, and inside a captive gap it works as a thrust washer or bushing (almost always what you want), or you give it a way out. Never leave a thin loose skin where it can work free and jam the joint.

Give it at least two layers (0.4 mm with 0.20 mm layers) so it survives the nozzle passing over it and keeps its shape. That thickness does not change the play: the washer touches both faces.

On vertical faces (a sleeve, a tooth flank) model between 0 and 0.1 mm per side and choose with a test coupon at 0 / 0.05 / 0.10 mm. Do not default to 0: the beads squash against the neighboring wall and can lock into its ridges even without bonding, and a sleeve modeled at zero can come out stiff. That range is a starting point, not a published figure.

A joint with no clearance runs on friction. For dry plastic on plastic, start from μ = 0.3–0.5 and then measure it; there is no published value for PLA on PETG. Washer wear and lubrication are in Friction and wear.

The bed has to suit both: PLA (35–65 °C) and PETG (60–80 °C) overlap at 60–65 °C. Each filament prints at its own nozzle temperature (PLA 190–230 °C, PETG 230–270 °C), each from its own profile. PP does not bond to the common filaments either (the table is in Functional multi-material parts). There are also breakaway interface materials made not to bond to PLA or PETG, such as Bambu's Support for PLA/PETG; they are meant to be peeled off and thrown away, so test one before you trust it as a working washer; PETG on PLA remains the place to start. A "PLA+" or "PETG" from an unknown brand may be a blend that does bond: let the coupon decide.

Soluble support inside the joint

Print-in-place clearances rules out supports inside a joint's gap: they weld or leave debris where you cannot reach. Soluble support is the exception. It can touch both faces because it disappears.

After the bath, a horizontal gap is as thick as the soluble layer was: one layer (0.2 mm instead of 0.4 with 0.20 mm layers), with a flat ceiling. You can also support overhangs inside a cavity, such as those of a ball joint or a captive part with an undercut. A student team at the University of Wisconsin–Madison printed PLA ball joints with PVA support on an Ultimaker 3, with 0.1 mm layers, and they worked with a 0.2 mm gap around the ball. It is a documented case, not a test series: its authors advise starting at 0.3 mm and working down.

The condition: water has to reach all of the soluble. Every pocket of soluble needs a path to the outside. In an annular gap open at the rim and at the shaft hole, PVA dissolves; in a sealed cavity, it does not. The water channel is drawn in Support materials.

PLA pairs with PVA. PETG and higher-temperature materials pair with BVOH, according to the manufacturers; check it with a coupon. ABS pairs with HIPS, which dissolves in limonene. Which soluble each part accepts is in Support materials. Dry PVA at 75–85 °C and BVOH at 60–80 °C, both for 8–12 h (Drying and storing filament).

If the gap is closed or you want zero play, use a non-bonding pair: it stays. If you want a real one-layer gap and water can get in, use soluble: it goes.

The cost: material changes

The slicer starts each layer with the material that finished the previous one. So a band of the second material that spans k layers costs about k changes, rounded up to the next even number: a one-layer band costs two, because the layer after it goes back to the base material. On a single-nozzle filament switcher, each change throws away about 0.2–0.8 g of purge depending on the colors (the average for Bambu's example cube is 0.54 g), and switching back to the part from support or another material usually takes more; count the changes before you print (Purge and multicolor waste). The cost is set by the layers the second material spans, not by how much of it there is.

A two-layer horizontal washer costs about 2 changes, and so does a one-layer band of soluble. A vertical sleeve 6 mm tall at 0.20 mm layers spans 30 layers: about 30 changes and some 16 g of purge. That is the second reason to put the second material on horizontal faces.

A toolchanger brings the bill down. For the INDX, Prusa quotes about 12 s and 13 mg per change: those 30 changes add up to about 0.4 g and about 6 min. The machines are in Toolchangers, IDEX and dual nozzles and Filament switchers: AMS, MMU, CFS and ACE.

Where the slicer allows it, purge into the part's infill or support, never into the visible walls of the turning body. What the option is called in each slicer is in Purge and multicolor waste.

30Vertical sleeve22Horizontal washersChangesVertical sleeve≈ 30Horizontal washers≈ 4Purge on a single-nozzle switcherVertical sleeve≈ 16 gHorizontal washers≈ 2 gLayers with two materials
Changes depend on the layers the second material spans. A vertical sleeve crosses all 30 layers of the lid; two horizontal washers, only four.

Worked example: a captive turntable

The part: a PLA lid, Ø60 mm and 6 mm thick, turning on a PLA base, held by a Ø10 mm pivot with a mushroom head. Vertical axis, printed in its working position. 0.20 mm layers, 0.4 nozzle, modern machine. There are two horizontal gaps: lid on base (thrust) and head on lid (retention). And one vertical gap: the pivot in the lid's hole.

With one material, each Z gap is one layer + 0.2 mm, so 0.4 mm. Axial play: 0.4 + 0.4 = 0.8 mm. Both ceilings are bridges. The underside of the lid spans 60 mm of air, three times the clean bridge of about 20 mm on a modern machine: expect it to sag until it touches the base and weld in places. The head's underside is prone to welding too. The hole gets 0.3 mm per side: Ø10.6 mm. Without a second material, the way out is to change the geometry: thrust faces as 45° cones, where 0.3 mm normal to the face becomes 0.42 mm vertically and there is no bridge.

With the non-bonding pair, both Z gaps become two-layer PETG washers (0.4 mm), modeled in contact with the PLA above and below. Axial play ≈ 0 and flat ceilings. The washers are trapped: they are the bearing the lid turns on. The hole keeps 0.3 mm of air per side. The bill on a single-nozzle switcher: 2 washers × 2 layers ≈ 4 changes, about 2 g. Bed at 60–65 °C.

If radial rattle matters too, add a PETG sleeve in the hole, at least two beads thick (about 0.8 mm of wall), leaving 0–0.1 mm per side between sleeve and pivot and between sleeve and hole, as the coupon says. The lid is 6 mm: 30 layers and about 30 more changes. That is about 16 g on a filament switcher and about 0.4 g on a toolchanger. Whether it is worth it depends on the machine.

With soluble, PVA goes in both Z gaps, one layer in each. After the bath each gap is 0.2 mm: 0.4 mm of axial play, half the single-material figure, and flat faces. Both gaps open to the outside, at the rim and toward the hole, so the water gets in. The bill: two one-layer bands at different heights, about 4 changes, the same as the washers. Bathe as the soluble's manufacturer directs and dry the part fully before judging how it turns.

The turntable in three versions
Version Z gaps Axial play Ceilings Changes, no sleeve (single-nozzle switcher)
One material 0.4 + 0.4 mm of air 0.8 mm sagging bridges 0
PLA + PETG washers 2-layer washers, in contact ≈ 0 flat ≈ 4 (≈ 2 g)
PLA + PVA 0.2 + 0.2 mm after the bath 0.4 mm flat ≈ 4 (≈ 2 g or a little more)
Turntable printed in gray PLA with the lid turned relative to the base and a thin orange line of the second material between lid and base
Turntable printed in gray PLA with the lid turned relative to the base and a thin orange line of the second material between lid and base

Rigid and TPU in one moving part

In a print-in-place mechanism, TPU is the part that bends or seals, bonded or keyed to the rigid parts; never one face of a gap that moves. TPU handles a print-in-place gap badly: it strings and sags, and it also partly bonds to PLA. An air gap between TPU and PLA combines the worst of both.

Typical uses:

  • A TPU strip as a hinge between two rigid plates. TPU survives more than 2 × 10⁶ folds; notches and creep limit it. Orient the beads so they cross the fold. Sizing is in Living hinges and flexures.
  • A TPU return spring or detent pad inside a rigid button or latch (TPU and lattice springs).
  • A TPU seal in a lid printed in place (Printed TPU gaskets).
  • TPU tires or jaw pads on rigid parts printed in place.

A TPU element is loaded on every cycle, often in peel from its ends, and against PLA, adhesion alone is not enough. Rigid and TPU hold mainly by mechanical interlocking: key it into the rigid part or let the slicer interlock the two materials; the bond figures per pair are in Functional multi-material parts.

Orient the part so the boundary between rigid and TPU is vertical (both materials side by side in every layer) and the bending span lies in the layer plane (Layer orientation for mechanisms). If they have to stack, rigid below and TPU on top: Prusa warns that rigid layers printed over a few layers of TPU shift sideways.

Which machine it takes: soft TPU needs a short path with a direct-drive extruder, which means a toolchanger or a second nozzle with direct drive. As of late 2026, on a single-nozzle filament switcher only a hard TPU made for switchers works in practice (Bambu's TPU for AMS is Shore 68D). The machines, purge and drying are in Functional multi-material parts; hardnesses and profiles in TPU and flexible filaments.

When it fails

Switcher jams and color streaks belong in Multi-material failures. Here, only the joint's.

Symptom, cause and fix
Symptom Cause Fix
The joint comes out welded even though it is PLA/PETG One of the two is a blend that does bond, or the second-material layer is narrower than one bead: the slicer dropped it and the ceiling sagged unsupported Coupon with the actual spools; check in the preview that the second material appears in every layer of the gap
The zero-clearance joint is too stiff to turn Beads locked into the ridges of the neighboring wall; elephant's foot at the bed edge Model 0.05–0.10 mm per side as the coupon says; 0.5 mm × 45° chamfer at the bed edge
Something rattles loose inside after a few turns A non-bonding skin has come free and is not trapped Make it a captive washer or sleeve, or remove it from the design
The joint stays stiff after the bath PVA trapped in a closed pocket Give every soluble gap a way out; longer bath in warm water; dry before judging
Purge is far higher than expected The second material spans many layers (vertical sleeve) Move it to horizontal faces or print on a toolchanger
The TPU element tears off at one end after a few cycles Peel at the end of a butt joint with PLA Key or interlock it, round the rigid corner or use PETG as the rigid material
The rigid layers shift on the TPU Rigid printed on top of a few layers of TPU Rigid below, TPU on top

How to test it

Before the part, the coupon: five short turntables (four if you have no soluble), or hinge sections, on the same plate. One with the single-material air gap, three with the non-bonding pair at 0 / 0.05 / 0.10 mm per side and one with soluble. Same spools and same profile as the part. Turn each by hand: it should be free, smooth and quiet. The general method is in Test coupons.

For TPU, the 10-minute strip test from Functional multi-material parts: bars overlapped 10–15 mm, plain, interlocked and keyed; test each in shear and in peel.

Then the cycles. A mechanism with a trapped washer or a TPU strip is judged after a few hundred cycles, not on the first turn; the method is in Testing a mechanism before you trust it.

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?