kapy academy

Friction and wear

18 min readUpdated Nov 2026

A printed pulley turns on an 8 mm steel shaft in a hole printed in the pulley itself. On day one it spins smoothly; after a weekend of running it squeaks, sheds dust the color of the part and wobbles: the hole has worn oval. Before you design a sliding pair, work out how much it rubs (μ), how hot it gets and how fast it wears (pressure, speed and distance), and decide whether grease or a change of material is enough, or whether the shaft needs a low-friction filament, a bushing or a bearing.

The friction coefficient is a range

The friction force is F_f = μ·N: the coefficient times the force pressing one surface against the other. There are two coefficients. The static one, which you have to overcome to get moving, is larger than the kinetic one, which acts while the surfaces slide. Because of that gap, one plastic sliding slowly over another jerks and squeaks: it sticks, jumps, sticks again. That is stick-slip.

Indicative friction coefficients
Pair μ
Printed PLA or PETG on itself, dry 0.3–0.5
Printed PLA or PETG on steel, dry 0.2–0.35
PA or POM on steel, dry 0.1–0.25
Low-friction filament on steel, dry 0.1–0.2
Greased plastic, or plastic with PTFE 0.05–0.15
Ball bearing (rolling) 0.001–0.005 (count on 0.005, the high end), plus the drag of its rubber seals if it has them
printed PLA/PETG on itselfPLA/PETG on steelPA or POM on steellow-friction filament on steelgreased plastic or plastic with PTFEball bearing ≤ 0.00500.10.20.30.40.5friction coefficient μ0°5.7°11.3°16.7°21.8°26.6°friction angle φ
Indicative ranges, dry and greased: start here and measure your own pair. Below, the friction angle that matches each μ.

They are ranges because a printed surface is not smooth: it is all beads and layer ridges. μ shifts with load, speed, temperature, humidity (in nylon), running-in and the finish of the other part. Anyone who gives you a single number for "PLA on steel" is giving you the number for their part, not yours. A ball bearing is not "almost zero" either: it rolls at μ of 0.001–0.005, but at low speed and on start-up the drag of its rubber seals can exceed that of a good PTFE bushing.

Every μ has a friction angle, φ = arctan μ: 0.1 gives 5.7°, 0.2 gives 11.3°, 0.3 gives 16.7°, 0.4 gives 21.8° and 0.5 gives 26.6°. A ramp, wedge, thread or cone is self-locking when its angle sits below φ. The same comparison sizes a self-locking worm or lead screw (Worm drives, Lead screws), the ramp of a detent (Ball and spring detents) and a cone clutch that will not let go (Friction and centrifugal clutches). Dry, plastic on plastic gives φ of 17–27°, and plastic on steel 11–19°. Compare a worm's lead angle λ with φ under real conditions, grease included: greased, μ ≈ 0.05 gives φ ≈ 3°, and a 5° worm that locked when dry stops locking. And a drive that does not back-drive at rest will not necessarily hold when it vibrates: under vibration, it creeps.

Sometimes friction is the function rather than the loss: a Friction hinge, Torque limiters, or V-belts and round belts, whose transmitted force grows with e^(μθ). This article is about the friction that wears parts and heats them.

What raises or lowers the friction of a printed part

The pair. Like against like (PLA on PLA, POM on POM) sticks, squeaks and wears faster. Two different materials do better, and hard, smooth steel against plastic is the best unlubricated pair you have to hand.

The other part. Use ground or precision rod. Never use threaded rod as a shaft: the thread acts like a file and eats the hole. Aluminum is soft and fiber-filled plastics score it, as they score a printed mating part (Carbon and glass fiber filaments).

The surface and orientation. Sliding along the beads is smoother than sliding across the layer ridges. A hole or pin with its axis vertical (Z) bears on the walls (perimeters) and comes out round. A pin printed lying down rubs against the layer ridges and comes out oval, with a sagging roof. The vertical pin wins on roundness and wear, but a bending load acts across its layers, which makes it the weakest: a trade-off between the two (Layer orientation for mechanisms).

Running-in. The first hours flatten the ridges: μ drops and the clearance grows by whatever has worn away (Clearances for moving parts). The debris stays between the two parts and keeps filing them unless you clean it out. A rubbing face that has been sanded or smoothed starts out almost run in (Sanding and smoothing).

Humidity and heat. Nylon absorbs water, swells, and changes its μ and its clearance (Nylons and polyamides). And every plastic softens under the heat of its own friction.

Wear and heat: pressure, speed and distance

A plain bearing is sized with three numbers:

  • Projected pressure: p = F / (d·L) (MPa, with F in N and d and L in mm).
  • Sliding speed: v = π·d·n / 60,000 (m/s, with d in mm and n in rpm).
  • Their product, PV = p·v (MPa·m/s).
FLdradial load Fprinted hubsteel shaftprojected area d × Lp = F/(d·L)Fn, rpmsliding speed vfriction μ·Fv = π·d·n/60,000P = μ·F·v
Pressure spreads over the projected area d × L; the heat depends on μ·F·v and not on the length of the bushing.

To a first approximation, wear follows Archard's law: the volume lost is proportional to load times sliding distance. Spread that volume over the area and the depth the hole loses is proportional to p times distance. Double the length of the bushing and the pressure halves, and so does the radial wear.

Heat is a separate calculation. The friction power is P = μ·F·v, in watts, and it does not depend on length. That heat decides whether the plastic softens: the part must stay below its service temperature under load, about 15–20 °C below its HDT at 0.45 MPa: PLA about 40 °C, PETG 50, ABS 70, ASA 80, PC 95 (Heat, cold, sunlight and chemicals). A smaller diameter lowers v, the heat and the friction torque (T = μ·F·d/2), but raises p: if heat governs, reduce d; if wear governs, lengthen L.

Molded or sintered bushings have a published PV limit. Treat it as a ceiling, never as the value for a printed part:

PV limits of molded or sintered plain bearings (Machine Design, “Bearings that bear up”)
Material Max PV (MPa·m/s) Max p (MPa) Max v (m/s)
Acetal (POM) 0.10 5 3
Unfilled PTFE 0.04 3.4 0.3
Filled (reinforced) PTFE 0.53 17 5
Oil-impregnated sintered bronze 1.8 28 6.1

There is no published PV for printed PLA, PETG or PA. A hole with layer ridges takes less than a molded part of the same polymer; the heat and wear you measure have the final say.

The big difference between a hinge and a shaft is the distance traveled. A Ø5 pin that opens 90° and closes ten times a day covers 7.85 mm per cycle: about 143 m in five years. A Ø8 shaft at 300 rpm covers 452 m an hour, 45 km in 100 h. The same plastic travels three hundred times as far in four days of continuous running.

Worked example: a Ø8 shaft at 300 rpm

The pulley from the start. The printed hub turns on an 8 mm ground steel shaft, in a hole 12 mm long (L = 12 mm, which meets the usual ratio L ≥ 1.5·d). Belt tension puts a radial load of F = 30 N on the shaft. It turns at n = 300 rpm, several hours a day.

  • p = 30 / (8 × 12) = 0.31 MPa.
  • v = π × 8 × 300 / 60,000 = 0.126 m/s.
  • PV = 0.039 MPa·m/s: 40 % of the ceiling for molded acetal, and that with a printed hole, rougher than any molded part.

With PLA on steel, dry, μ = 0.3: P = 0.3 × 30 × 0.126 = 1.1 W continuous. Now the temperature, worst case: a hub with about 30 cm² of surface in still air (about 10 W/m²·K) rises about 35 °C above ambient at 1.1 W. Some of the heat leaves through the steel shaft, so this is an overestimate, but the order of magnitude puts the PLA at 55–60 °C, well above its 40 °C under load. Friction also costs the shaft T = 0.3 × 30 × 4 = 36 N·mm of torque.

Same load, same speed, four solutions
Solution μ Heat P Torque lost T Note
Printed PLA hole 0.3 1.1 W 36 N·mm heats up and goes oval
Low-friction filament 0.15 0.57 W 18 N·mm better, but still plastic
Oil-impregnated sintered bronze bushing 0.1 0.38 W 12 N·mm runs at 2 % of its PV limit (1.8)
608-ZZ bearing (shielded, no contact seal) 0.005 0.02 W 0.6 N·mm negligible heat; a 608-2RS adds the drag of its seals, which at this load can exceed the rolling friction

Lengthening the PLA hole to 24 mm halves p and the wear rate, but the heat is still 1.1 W. This shaft calls for a bronze or polymer bushing, or a bearing, not the printed hole. Pick the size in Standard bearings and bushings and seat the bushing or bearing as described in Seating bearings and bushings.

Compare it with the hinge of a lid: a Ø5 pin, L = 10 mm, 5 N. p = 0.1 MPa, it moves at hand speed, and it covers 143 m in five years. The heat is negligible and the wear slow: a printed pair with a little silicone grease is enough.

Lubricants: which one for each plastic

With plastic, the risk from a lubricant is environmental stress cracking: a chemical that would do nothing to an unstressed part cracks a stressed one, such as a press fit, a clip, a screw boss or the residual stress from printing. PC is the most sensitive, then ABS and ASA. The crack can appear days later and away from where you can see the grease.

Lubricants and printed plastics: starting points to test
Lubricant Verdict Why
Silicone grease first choice on PLA, PETG, ABS, ASA, PC, PA and POM attacks almost none of them; leaves the surface impossible to glue or paint
Plastic-safe PTFE grease (PAO or silicone base) also a first choice the label must say it is plastic-compatible
Dry PTFE spray for dusty settings: it does not turn to paste let the solvent evaporate before loading the part; test it on PC
Graphite powder dry, though it marks conducts electricity
Mineral or lithium oils and greases fine on PA, POM and nearly always PLA never on PC; avoid on stressed ABS and ASA
Synthetic ester-based oils and greases avoid act as slow solvents on ABS and PC
Penetrating oils and water displacers (classic multi-use WD-40, for example) not mechanism lubricants they are solvents that strip grease and attack PC

On PP, hydrocarbon oils can swell the part slightly: start with silicone. The same cautions apply to anaerobic threadlockers and retaining compounds: they cure poorly on plastic and can crack ABS and PC. To fix a bushing in a printed part, use cyanoacrylate or epoxy (on PC, epoxy only: cyanoacrylate cracks it too and leaves a white bloom), or a retention feature designed into the part. Degrease the outside of the bushing and keep the adhesive out of the bore. A sintered bronze bushing is not greased: grease blocks its pores and cuts off the oil. If it needs topping up, add a few drops of oil.

Apply a thin film. Grease traps dust and print debris and becomes an abrasive paste; on an exposed guide a dry lubricant (PTFE spray) lasts longer. Set the greasing interval from your own tests; do not wait for it to squeak. Before trusting a lubricant on PC or ABS, apply it to a part under the same stress it will see in use (a clip held open, a pressed-in pin), wait 48 h and look for whitish microcracks. If the part touches food, see Printing for food contact. Chemical resistance data is in Heat, cold, sunlight and chemicals.

Low-friction filaments: when they pay for themselves

These filaments are a base polymer (PA, PETG or a maker's own blend) loaded with solid lubricants: PTFE, graphite, MoS₂ or PTFE-free additives. Plain nylon is not self-lubricating; the filled grades are (Nylons and polyamides).

As of late 2026, the benchmark is igus's low-friction (tribological) filaments, the iglidur range: i180-PF and i190-PF, the latter PTFE-free, with a maximum service temperature of 90 °C once annealed. Several makers also sell PETG with 10 % PTFE. The EU is processing a broad PFAS restriction, which is why PTFE-free grades are gaining ground.

The wear data comes from the manufacturer: igus claims up to 50 times less wear than a standard filament in its pivoting test against ABS and, for i180-PF, 15 times less than ABS in a linear test. There is no independent data on printed parts to compare them. And they cost a good deal more than a standard spool.

They pay off when the printed part itself has to be the sliding surface and there is no room for a bushing: gear teeth, a lead-screw nut, a cam follower, a custom-profile slide or an oddly shaped bushing. There μ roughly halves (0.1–0.2 against 0.2–0.35 on steel), and the wear is whatever your tests say. They do not pay off in a round hole that will take an 8 × 12 bronze bushing: the bushing wins on μ, on PV and on price.

Dry them before printing, as the datasheet specifies. Some need an enclosed printer and an adhesive on the build plate. If only the contact surface needs the low-friction material, print that zone in it and the rest in standard filament (Multi-material print-in-place). Fiber-filled grades wear a soft mating part: run them against hardened steel.

Plastic, bushing or bearing

diagram
From a printed pair to a ball bearing: move up a step when speed, hours or heat demand it.

A printed pair with silicone grease is enough for anything that moves slowly, now and then, over a short distance: hinges, knobs, latches, toys, anything worked by hand. Check the pressure and that it does not heat up.

A bushing, oil-impregnated sintered bronze or polymer, is for continuous rotation or oscillation at moderate speed, with dirt or shocks, or on a tight budget. It needs a smooth steel shaft; lubricated, it gives μ of 0.05–0.15, and you check its PV against the catalog. For linear motion, the 2:1 rule and L ≥ 1.5·d are in Rod and linear bushing.

A ball bearing is for high speed, long hours, precision or low breakaway torque. It gives μ ≤ 0.005 plus the drag of its rubber seals. Linear ball bearings need hardened rod (Rod and linear bushing), and every bearing needs a housing that does not squeeze it (Seating bearings and bushings). For the material of the part that houses it, see Which plastic for which mechanism.

When it fails

Two identical printed pulley hubs in gray PLA, seen from above: on the left a new one, its hole round with a clean edge; on the right one after hours on a steel shaft, its hole worn oval to one side, the wall on that side polished and shiny, and dust the same gray as the part around the mouth of the hole and on the table
Two identical printed pulley hubs in gray PLA, seen from above: on the left a new one, its hole round with a clean edge; on the right one after hours on a steel shaft, its hole worn oval to one side, the wall on that side polished and shiny, and dust the same gray as the part around the mouth of the hole and on the table
What usually goes wrong in a sliding pair
Symptom Cause Fix
Squeaks or jerks when moving slowly stick-slip: like-on-like pair, dry silicone or PTFE grease; change the material of one of the two parts
Dust the color of the plastic and play that grows within days the part is wearing: rough shaft (threaded rod), ridges across the motion or too much travel ground rod, beads along the motion, a bushing
Gray or black metallic dust the shaft is wearing: abrasive fiber or a soft shaft (aluminum) hardened steel shaft or an unfilled grade
The hub feels warm, then seizes and the hole goes oval friction heat above the service temperature lower μ·F·v: smaller diameter, bushing or bearing, or a more heat-resistant plastic (ASA, PC)
A crack appears near the grease days later environmental stress cracking plastic-safe silicone or PTFE grease; 48 h test
Tight on humid days, loose on dry ones nylon absorbs water more clearance, PA12 or filled PA (they absorb less), or another material
The grease turns into a gray paste dust and print debris clean, apply a thin film or dry PTFE, and shield the joint from dust
Fine at first, rough after an hour running-in debris trapped in the joint clean and re-lubricate after running-in

How to test it

Static μ by tilting. Rest a printed block on a plate of the other part's material. A block, never a ball or a cylinder: they roll. Lift one end slowly until it slides: μ = tan θ. Your phone's inclinometer will do. 17° is about 0.3; 6°, about 0.1.

Kinetic μ. Drag the same block at constant speed with a spring balance or a cheap digital force gauge: μ = drag force / weight. Measure three times dry and three times greased.

Wear and heat on the real joint. Spin it with a drill or its own motor for 1 h, measure, and carry on to 10 h. Measure the play with gauge pins or feeler gauges, and the hole diameter. Take the hub temperature with an infrared thermometer and compare it with the plastic's service temperature. The debris is no use for quantifying wear: 0.1 mm of wear over half of a Ø8 × 12 hole is about 20 mg of PLA. If you want a figure by mass, weigh the part before and after on a 0.001 g scale.

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?