A coil spring or a leaf spring responds in a straight line: the further you deflect it, the harder it pushes, always in the same proportion. Plenty of jobs want a different curve: a seat, a soft first touch and a firm finish; a button, the same force at the top and the bottom; a wind-up toy, torque over several turns. That shape comes from geometry. With TPU or a TPU lattice you can print it, for a few newtons; a printed spiral gives light torque, and the constant-force spring is bought in steel.
Four curve shapes and where each comes from
Before you design, decide which curve you need. Four shapes are within reach of a printer or a catalog, and each comes from a different physical mechanism.
- Linear. A beam working in bending: the leaf spring, the cantilever, the coil spring (Leaf and cantilever springs, Coil springs). Force rises in proportion to deflection.
- Progressive (stiffening). A TPU pad bonded on both faces, which gets stiffer as it thins; a graded-density lattice, where the soft layer gives first; or a second spring or a stop that comes into play halfway through the stroke.
- Regressive to a plateau. A column or a cell wall that buckles. The force rises, stays almost flat, then shoots up when the cells touch: that is densification. Once bowed, the column works in bending at an almost constant force, and that is where the plateau comes from.
- Constant. A pre-formed strip unrolling from a drum. The strip only changes curvature over a short stretch, always the same length, so the force does not depend on how much you have pulled out.
There is a fifth shape, negative stiffness, where the force drops as you advance and the part snaps through. That belongs to Compliant bistables and Snap domes.
In a TPU spring the unloading curve always runs below the loading curve. The area between them is the hysteresis: energy lost as heat on every cycle. In a damper that is what you want; in a return spring it is force you do not have on the way back. Measure the loop as described in Testing a mechanism before you trust it.
TPU: lots of travel, little force
A spring in rigid plastic is limited by the allowable strain: in repeated use PLA takes 1–1.5 % (1 % if it is actuated daily) and PETG 2 % (Print-friendly snap fits). TPU has no such ceiling at those levels; notches and creep limit it instead. A TPU living hinge survives more than 2 million folds, a job no printed rigid plastic can take.
The trade-off is modulus. For TPU 95A, calculate with E ≈ 9 MPa (Bambu's datasheet gives 9.2 in XY); PLA's design E is 2.5 GPa. The same blade in TPU gives roughly 280 times less force. Other TPU 95A datasheets give very different figures depending on the test, so moduli are not comparable between brands: allow ±50 % and measure. A TPU spring is good for a few newtons over millimeters of travel. If you need 20 N in a small space, the spring is steel: Using bought steel springs.
TPU gives in three ways, bending, solid compression and buckling (the mechanism of each is explained in Designing flexible parts). What matters here is the curve each one produces:
- Bending: a straight line, like any leaf spring.
- Pad bonded on both faces: a progressive curve. A pad held at top and bottom cannot bulge freely at the sides, and the thinner it is, the less it can. The shape factor S measures this: the loaded area divided by the free side area. The effective compressive modulus follows Ec ≈ E·(1 + 2k·S²), with k ≈ 0.5–1. It is an empirical rule from rubber, not validated on printed TPU, and it assumes a solid pad at 100 % infill: with partial infill the pad is no longer incompressible and S no longer applies. Trust the trend, not the number.
- Buckling blades: a plateau.
| Ø20 mm pad | Shape factor S | Effective modulus Ec/E |
|---|---|---|
| 10 mm thick | 0.5 | ≈ 1.25–1.5 |
| 2 mm thick | 2.5 | ≈ 7–13 |
That is why a pad stiffens as it is squashed: as it thins, its S grows. And its stiffness grows faster than its modulus, because it also scales with 1/h: going from 10 to 2 mm thick, that term alone multiplies it by five.
To make a blade buckle toward the side you choose, give it a pre-bow of 5–10 % of its length toward that side, or offset its support slightly. It then always buckles that way, with a lower, rounded force peak, and the blades do not collide. A perfectly straight blade picks its side at random and gives a peak followed by a drop: under a finger it feels like a click.
The real limits of a TPU spring are hysteresis and time. Held compressed, it relaxes and loses force within hours, faster when warm (Creep and fatigue). In the cold it gets stiffer. So size a TPU return spring on the unloading curve measured after 48 h in the working position, not on the first day's loading curve.
Start with TPU 95A and drop to a softer grade only when you cannot thin the geometry any further. The 68D "TPU for AMS" is a different class of material: semi-rigid, more than a hundred times stiffer than the same brand's TPU 95A (1190 MPa against 9.2 in XY) and far less elastic in Z than in XY. Do not use it for a large-deflection spring. Grades, Shore hardness and how to print them are in TPU and flexible filaments.
Worked example: a TPU blade spring for a button
The brief: a return spring under a 25 mm button. You want an almost flat force of about 8 N over 3 mm of travel, so the button feels the same at the top and the bottom. Material: TPU 95A. Two opposed blades.
The geometry: the first instinct is a short blade, L = 10 mm. Over 3 mm of travel that blade shortens by 30 %, bows out about 3.5 mm and its surface works at 40 % strain on every press, at the root and at the center. TPU takes it, but hysteresis, relaxation and tearing at the root all grow with strain. Lengthen the blade until the travel is around 20 % of L:
- thickness t = 1.2 mm (3 lines),
- free length L = 14 mm,
- starting width w = 8 mm,
- fixed at top and bottom, pre-bowed outwards, with a fillet of r ≈ 0.6 mm (0.5·t) at both roots.
With L = 14 mm and 3 mm of travel, the surface strain drops to 25 %.
The orientation: print the spring lying down, with the button axis horizontal. L and the bending then sit in XY, the strain runs along the beads and w is the wall height in Z: stance B, the best one (Layer orientation for mechanisms). Standing up, with the button on top, the blade would run in Z and work across the layers.
The prediction: the buckling load of a column fixed at both ends is P = 4·π²·E·I/L², with I = w·t³/12 = 8·1.2³/12 = 1.15 mm⁴. That gives P ≈ 0.23·E per blade (E in MPa, P in N). With E = 9 MPa, 2.1 N per blade and 4.2 N for the pair. With another TPU, the result scales with its modulus. The formula tells you how the force varies; the test piece gives you the value.
Nor is the plateau perfectly flat. A fixed-end blade that shortens by 20 % pushes about 10 % harder at the end than when it starts to buckle (the ideal elastica gives +11 %; real TPU can climb a little more). If 8 N is the minimum, you will have about 9 N at the bottom.
The test piece: print three pairs of blades with t = 0.9, 1.2 and 1.6 mm: 2, 3 and 4 whole lines, with no fractional widths for the slicer to fill with variable-width lines. The plateau force is proportional to t³: factors 0.42, 1 and 2.37. Say the 1.2 mm pair reads 5.5 N at the start of the plateau (an example reading, not data). Keep t at 3 lines and adjust with the width, which is linear and independent of line count: w = 8·(8/5.5) ≈ 11.6 mm.
| Parameter | Effect on force | Use |
|---|---|---|
| Thickness t | ∝ t³ | coarse adjustment, in whole lines |
| Width w | ∝ w | fine adjustment, linear |
| Length L | ∝ 1/L² | large change; more L, less strain for the same travel |
The travel: each blade bows out about 4 mm with the button fully pressed (a ≈ √(4·L·Δ)/π, with Δ the travel). Leave room for that bow plus at least 1 mm of air to the housing, and keep the blades from touching each other. If the gap is smaller, the blade hits early and the curve shoots up against the wall. A separate hard stop is what should limit the travel.
The return: on the unloading curve, the force 0.5 mm from the end of travel must still exceed the button's friction plus its weight. If the button stays pressed (a latching push button), measure that force after 48 h held down.
Lattices: stiffness comes from density
A lattice is a network of small springs, in series and in parallel. Its stiffness is set mainly by relative density ρ*/ρ, the fraction of the volume that is material. Gibson and Ashby give the scaling laws, with E* and σ* the modulus and stress of the lattice and E that of the solid material:
| Quantity | Expression | What it means |
|---|---|---|
| Stiffness (struts in bending) | E*/E ≈ (ρ*/ρ)² | double the density, four times stiffer |
| Stiffness (struts in tension or compression) | E*/E ≈ (ρ*/ρ)/3 | double the density, twice as stiff, until they buckle |
| Plateau stress (elastic buckling) | σ* ≈ 0.05·E·(ρ*/ρ)² | the plateau force |
| Densification strain | εD ≈ 1 − 1.4·ρ*/ρ | at 20 % density, useful travel ends at about 70 % of the height |
Printed cells stray from these formulas; what is useful is the exponents. Densification, here, is the spring's end of travel. Designing a lattice to absorb an impact is a different problem, covered in Shock-absorbing lattices.
With graded density, the progressive curve comes made to order. Stack three layers at 10, 20 and 30 %. Their stiffnesses go as 1 : 4 : 9. The soft layer collapses first, then the next: a staircase that in the real part rounds off into a progressive curve. Use it for the padding of a seat or a handle, soft at first touch and firm at the end, or for the pad of a gripper.
A rigid lattice is not a spring. In a PLA lattice with struts in bending, the strut strain is of the order of 3·(t/l) times the overall strain, with t/l the strut's slenderness (thickness over length), 0.2 to 0.3 in printed cells. The strut reaches PLA's allowable 1 % when the whole part has been compressed by 1–2 %: in a 20 mm block, 0.2–0.4 mm of travel. If you need travel in a rigid material, lengthen the beam by folding it into a Serpentine flexure or use a leaf spring. Use the rigid lattice as a lightweight structure.
There are two ways to make the lattice:
- Slicer infill, with no top or bottom layers. The cheap route. Patterns, walls and why switching slicer profile changes the part are explained in Designing flexible parts and Walls, perimeters and infill.
- Modeled cells, when you need direction, grading or an exact strut. In TPU: struts at least 2 lines wide (0.9 mm with a 0.4 nozzle), self-supporting cells with struts at 45° or less from vertical and no horizontal bridges, because bridges sag in TPU. Round the nodes: tearing starts at sharp inside corners.
Layer bonding is not the limit here: a TPU 85A keeps about 88 % of its XY strength in Z. Directional, auxetic and minimal-surface cells are in Auxetics and lattices. For a TPU lattice printed onto a rigid plate, see Functional multi-material parts and Multi-material print-in-place.
Clock spiral and constant-force spring
An open spiral, with the coils not touching, is a long beam in uniform bending: its torque rises in a straight line with angle, M = E·b·t³·θ/(12·L), and the surface strain, ε = t·θ/(2·L), sets the turns (b the width, t the thickness, L the strip length and θ the rotation in radians). With t = 0.9 mm, b = 6 mm and L = 600 mm, it gives about 2.1 turns and 20 N·mm in PLA (1 %, design E 2.5 GPa) and about 4.2 turns and 26 N·mm in PETG (2 %, 1.6 GPa): 0.2–0.26 N on a 100 mm arm, for a toy, the return of a pointer or a reel taking up a thin cord. Print it flat, with the strip as a vertical wall that flexes in XY, the inner end joined to the arbor with a fillet of r ≈ 0.5·t and a gap between coils larger than the amount each one closes up when fully wound. Do not leave it wound: it relaxes and loses torque within days. Winding, gear trains and the escapement are in Spring motors and flywheels.
A constant-force spring is a strip formed to a natural radius Rn and wound onto a drum. When you pull, it always straightens over the same short stretch, so the force is flat, of the order of F ≈ E·b·t³/(26.4·Rn²) according to manufacturers' calculators. Printed, it does not work: with PLA's 1 %, Rn ≥ 50·t, and with t = 0.9 mm and b = 10 mm you get a 90 mm roll that gives ≈ 0.34 N; left extended, it also relaxes and loses the curvature its force depends on. A stainless steel one with b = 10 mm, t = 0.1 mm and Rn = 5 mm gives ≈ 2.9 N from a roll about 12 mm across. Buy it in steel and print its drum and mount (Using bought steel springs): catalogs put the drum 10–20 % larger than the spring's natural diameter, and the force only becomes constant after an initial extension of about 1.25 times the roll diameter. If you need an almost flat printed force, use buckling TPU blades, as in the button example.
When it fails
| Symptom | Cause | Fix |
|---|---|---|
| The TPU spring is much stiffer or softer than calculated | The modulus of that brand and grade, or a different slicer profile | Test piece with three thicknesses in whole lines, adjust with the width, and note the profile next to the model |
| Pressing gives a peak then a drop (a click) | Straight blade buckling to a random side | Pre-bow of 5–10 % or an offset support |
| Returns slowly or does not reach the top | Hysteresis and relaxation; sized on the loading curve | Size on the unloading curve after 48 h; longer, less strained blades |
| The blade tears at the root | Excessive strain and a sharp corner | Travel around 20 % of L; fillet r ≈ 0.5·t |
| The curve rises early | Blades hit the housing or each other; in a lattice, densification | Gap for the bow plus 1 mm of air; lower density |
| A cell sagged during printing | Bridges or overhangs beyond 45° in TPU | Self-supporting cells, thicker struts |
| A PLA lattice cracks at the nodes after a few presses | Rigid lattice used as a spring | TPU, or a serpentine or a leaf spring |
| The spiral loses torque within days or the coils rub | Creep while wound; too little gap between coils | PC or ASA; wind it less or let it unwind at rest; more gap; if it sits wound for days, a steel spring |
| The printed constant-force strip loses force | Relaxation: the natural radius grows | Bought steel strip |
How to test it
Measure the force-travel curve on loading and unloading with the screw-and-scale rig, hold the spring in its working position for 48 h and measure again. The rig and the test are in Testing a mechanism before you trust it. A return spring passes when its unloading force at the end of travel comfortably exceeds the friction plus the weight of whatever it returns.
See also
- Using bought steel springs: when a linear curve is enough and what you lack is force.
- Compliant bistables: negative stiffness, when the part has to snap.
- Shock-absorbing lattices: a lattice for an impact rather than a spring.
- Spring counterbalancing: an almost flat force from an ordinary spring and a geometry that compensates for it.