kapy academy

Printed TPU gaskets

19 min readUpdated Nov 2026

Print a TPU gasket in the exact shape of your rim when the box only has to keep out rain, dust or splashes. It seals if the geometry fixes the squeeze and the lid rim is stiff enough to hold that squeeze between one screw and the next. Printed, the gasket has no splice and can be fused to the part; in exchange, TPU loses squeeze over time and with heat. For pressure, heat or years closed, buy an O-ring (O-ring grooves).

Three ways to seal with TPU

No stopLidGasketRimFlat gasketStopSqueezeLidGasketRimGroove with stopInterferenceWaterLidRimGasketLip
Where the squeeze comes from in each case. Without a stop, the screwdriver decides it. With a groove and a stop, the model decides it. A lip loads itself as it bends.

Flat gasket, no stop. The easiest to draw and the worst performer. Next to each screw it is over-squeezed and squeezes out of the gap; between screws it barely touches. And when the TPU relaxes, the squeeze drops with nothing to hold it. Use one only with compression limiters: sleeves or bosses round each screw that let hard plastic bear on hard plastic, or a raised edge that acts as a stop.

Gasket in a groove, with a stop. The default for a printed box. The lid bears on rigid plastic, so the squeeze is how far the gasket stands proud of the rim: you choose it in the model, and it does not change however hard the screw is tightened. The groove dimensions and the maximum fill are in Designing flexible parts, with their figure.

Lip. A thin TPU flap that bends against a wall. It needs very little force and tolerates a lid that moves a little, so it is the only seal that works on a lid closed with clips. The trade-off: it yields to pressure from the other side, and dust collects under it.

Choose the stop first. A gasket whose squeeze depends on how hard a screw is tightened will leak on its second assembly.

How much to squeeze: flatness decides

For a static seal, compress the gasket by 15 to 30 % of its free height. These are O-ring figures (Parker ORD 5700) adapted to printed TPU, not a TPU standard. For a solid printed gasket, aim for 25 %. Below 15 %, the relaxation of the first few weeks leaves the gasket out of contact. Above 30 %, the force shoots up, because the material is nearly incompressible, and the compression set grows.

On a printed part, the squeeze in millimeters has to absorb two things at once. The first is lack of flatness: if a 120 mm lid warps or bows by a few tenths of a millimeter, somewhere there is a gap as wide. The second is the opening δ of the rim between two screws, which you will see in the next section. At the worst point, 15 % of the height h must still remain:

squeeze − bow − δ ≥ 0.15·h

With a nominal squeeze of 25 % of h, that gives squeeze ≥ (bow + δ) / 0.4. Measure the bow with a feeler gauge, with the lid on a flat surface. With 0.2 mm of bow and δ = 0.10 mm, the squeeze comes out at 0.75 mm and h = 3.0 mm, 15 layers of 0.20 mm. Measured free, the bow is pessimistic: the stop and the screws partly straighten the lid when you close it. But do not count on that mid-span, which is exactly where the lid opens.

The gasket height and the rim height are multiples of the layer height, and so is the squeeze (Clearances for moving parts).

You win flatness before you design the gasket. If the corners lift, the fix is in Warping and lifting corners; shrinkage is in Shrinkage and dimensional stability. And make the gasket seal on a top face or on the bed face, never against a stepped vertical wall, because there the layer lines cross the seal.

Which TPU: 85A or 95A?

With the same geometry and the same squeeze, the force is proportional to the modulus, and a 95A pushes about three times harder than an 85A (Gent's relation, as in Designing flexible parts). A softer TPU needs fewer screws and bows the lid less.

The other figure that matters is compression set: the percentage of the squeeze the gasket no longer recovers after being compressed for a while.

Compression set (ISO 815), from the Ultrafuse datasheets
Grade 23 °C, 72 h 70 °C, 24 h
Ultrafuse TPU 85A 26 % 52 %
Ultrafuse TPU 95A 38 % 90 %

After a day at 70 °C, as inside a car in the sun, the 95A gasket recovers only a tenth of its squeeze; the 85A, half. Even at room temperature, a 95A loses more than a third in three days: another reason for the margin in the previous section. These are one manufacturer's figures on its own specimens, and the datasheet does not say whether they were printed or molded. A printed gasket, with voids and layer lines, will not do better than those specimens.

Use 85A–90A if your printer can feed it (direct drive, short path; TPU and flexible filaments). If not, use 95A with less squeeze, around 20 %, and more screws. "AMS-compatible" TPU at 64D–68D will not do: it is semi-rigid, with a modulus of about 1190 MPa against about 9 MPa for a 95A. Nor will foaming TPU, which absorbs water and does not print to reliable dimensions. Both cases are explained in TPU and flexible filaments.

Temperature matters too. Cold stiffens TPU, so a gasket presses harder in winter; heat makes it relax sooner. If the gasket will run hot or spend years compressed, buy an O-ring or a molded gasket (Creep and fatigue).

Closing force and screw count

Closing force is measured per millimeter of gasket: q, in N/mm. For a solid strip you can estimate it with the shape factor S, the ratio of the loaded area to the area of the free sides, which bulge. For a long strip pressed from above and below, S = w/(2h). The effective compression modulus is Ec ≈ E·(1 + 2k·S²), with k between 0.5 and 1, the same expression as in TPU and lattice springs. The stress is Ec times the strain, and q is that stress times the contact width w. The expression assumes faces that do not slip; a loose gasket between smooth faces comes out softer. The formula gives the order of magnitude; the real value comes from a coupon, because TPU is designed with measured curves.

Estimated closing force at 25 % squeeze (TPU 95A: E ≈ 9 MPa; 85A: one third)
Gasket section S Ec q Over 400 mm of perimeter
Solid strip 3 × 3 mm, 95A 0.5 11–13.5 MPa 8.5–10 N/mm (≈ 9) ≈ 3.6 kN
Bead 1.2 × 3 mm, 95A 0.2 ≈ 10 MPa ≈ 3 N/mm ≈ 1.2 kN
Bead 1.2 × 3 mm, 85A 0.2 ≈ 3.3 MPa ≈ 1 N/mm ≈ 0.4 kN

Nearly four kilonewtons is more than a printed lid and a few M3 screws in plastic bosses can take without creep. Some 95A grades are stiffer, and moduli from different brands are not comparable: measure yours. The force grows with contact width and with E, but sealing needs continuous contact, not width. Before adding screws, narrow the contact: a thin bead, a rigid rib that bites into a flat 85A gasket, or a lip.

Opening δPitch pScrewLidGasketGasket load q (N/mm)Flat plateWith skirtI × 15
Between two screws, the lid rim works as a beam loaded by the gasket and opens in the middle. A skirt does more for the rim than any extra screw.

The stretch of rim between two screws is a beam fixed at both ends under a uniformly distributed load q, and at the center it opens by δ = q·p⁴ / (384·E·I). Here E is the modulus of the lid plastic, I the second moment of area of the rim and p the screw pitch. Solving for the pitch: p = (384·E·I·δ / q)^(1/4). Because of the fourth root, to double the pitch you have to divide q by 16 or make the rim 16 times stiffer; halving q lengthens it by only 19 %. The cheapest fix is to give the rim depth: I grows with the cube of the depth.

The screws go outside the gasket loop, on an outer flange or on lugs, or the gasket goes round each screw. A hole inside the sealed enclosure is a direct leak path, and an insert in an open boss is another. If a screw has to sit inside, make its boss blind, closed at the bottom, and put a sealing washer or an O-ring under the head.

Put a screw within half a pitch of every corner. At a corner the gasket turns and the rim is already stiffer, but a corner without a screw is the most common cause of leaks. Each screw carries q·p. If the box will be opened often, use heat-set inserts (Designing for heat-set inserts); if rarely, self-tapping screws (Self-tapping screws in plastic). Keep the permanent load on the bosses low, because the plastic creeps.

Worked example: a 120 × 80 mm box against rain

A PETG box for an outdoor sensor, 120 × 80 mm, with about 400 mm of gasket perimeter. It has to withstand rain and splashes, is opened a few times a year and closes with M3 screws in heat-set inserts, on a flange outside the gasket. Measured with a feeler gauge, the lid bows by 0.2 mm.

Squeeze and type. Set the allowable opening between screws at δ = 0.10 mm. Squeeze ≥ (0.2 + 0.10) / 0.4 = 0.75 mm; at 25 %, h = 3.0 mm, 15 layers. At the worst point, 0.75 − 0.2 − 0.10 = 0.45 mm remains, 15 % of h. It goes in a groove with a stop: the rigid rim is the stop. For the lid, the calculations use PETG's design modulus, E = 1.6 GPa (Which plastic for which mechanism).

Option A: a solid 3 × 3 mm strip of 95A, q ≈ 9 N/mm. A flat 3 mm lid; take a 10 mm strip next to the edge as the beam: I = 10·3³/12 = 22.5 mm⁴. p = (384·1600·22.5·0.10 / 9)^(1/4) ≈ 20 mm. That comes to about 20 screws and nearly 4 kN on the lid: with this section, no number of screws will work.

Option B: a 1.2 × 3 mm bead of 85A–90A in its groove. Assume the coupon reads 1 N/mm (an example reading, not data; it agrees with the table). With the same flat lid, p = (384·1600·22.5·0.10 / 1)^(1/4) ≈ 34 mm. That comes to about 12 screws.

Option C: the same bead, and the lid with a skirt 2.4 mm thick. Now the rim works on edge. At 12 mm high, I = 2.4·12³/12 ≈ 346 mm⁴, 15 times more, and p ≈ 68 mm. With the screws at the corners of the flange, about 5 mm from the outer edge, the spans come to about 55 mm on the long sides, with a screw in the middle, and about 70 mm on the short ones, which are slightly over. Raise the skirt to 13 mm: I ≈ 439 mm⁴ and p ≈ 72 mm. Six screws are enough, and each carries q·p, about 55–70 N (400 N in total), very little for an M3 insert.

Printing the gasket separately

Printed, the gasket is a single closed piece in the exact shape of the rim: it has no splice, the weak point of a cord cut to length and joined.

Print it flat, sealing face up, solid, with dry TPU (Drying and storing filament). Set the top surface pattern to concentric so the beads run along the gasket and no furrow crosses its width.

In a groove, the gasket also seals against the bottom, so both its faces seal. The troublesome one is the bed face: on textured PEI it copies the texture and leaves channels. You have three fixes: print it on a smooth plate, with glue stick as a release agent; add a sealing bead on each face; or print it onto the part, which removes that leak path (next section).

The Z seam leaves a bump or a notch on the gasket's side walls. On a face seal it does not cross the sealing face; on a radial seal, which seals on its side, it does. Avoid radial seals against printed vertical walls, or move the seam to the point of greatest squeeze. On the rigid face it seals against, ironing the top surface helps (Top surfaces).

Printing it onto the rigid part

Printed onto its rim or inside its groove, the gasket is fused to the part: the leak path underneath disappears and the gasket cannot fall out or go missing. For that you need a second extruder that can feed soft TPU. As of late 2026, that means a toolchanger or a second direct-drive nozzle. According to their makers, single-nozzle filament switchers do not accept TPU softer than about 68D, and the "AMS-compatible" TPUs that do get through are too hard for a gasket. Which machines can do it, and with what limits, is covered in Toolchangers, IDEX and dual nozzles and Functional multi-material parts.

Choose PETG for the rigid part: users report, though nobody has published measurements, that TPU bonds better to PETG than to PLA. A face gasket works only in compression, so the bond is barely stressed. The delicate moment is opening the lid: if the TPU has stuck to the opposite face, pulling the lid open starts peeling the gasket off its base from the edge. Make the opposite face smooth, and never leave the top face of the TPU textured.

With one nozzle there is another way: a single filament change at one layer height, with the same pause as in Embedding magnets and nuts mid-print. It only works if everything above that height is TPU, that is, with the gasket on a flat rim, no groove around it and nothing rigid carrying on upwards. The bond lies in a layer plane, the weakest, but it works only in compression: fine for a gasket, not for a lip that flexes. A gasket in a groove mixes rigid and TPU in the same layers and would need a filament change on every layer, which pauses cannot do.

Put the rigid material below and the TPU on top: a rigid part printed on a few layers of TPU shifts sideways while it prints. A lid printed upside down leaves its rim on top, ready to take the gasket. For TPU parts inside moving mechanisms, see Multi-material print-in-place.

Sealing lips

A lip is a short TPU cantilever pressed against a wall by interference. The contact force comes from bending, not from compressing the material, so it is very small and hardly depends on the tolerance. Per millimeter of lip, P/w = E·t³·y / (4·L³). A 95A lip of thickness t = 1.0 mm, length L = 3 mm and interference y = 0.6 mm gives about 0.05 N/mm, as an order of magnitude. That is why a lip seals against splashes and dust on a lid closed with clips: it is the exception to the "a clip does not clamp" rule in Enclosure lids.

TPU lip: starting dimensions
Dimension Value Why
Thickness t 0.8–1.2 mm, in whole layers thick enough not to fold over itself, thin enough not to need much force
Length L 3–5 mm the longer it is, the less force and the more tolerance
Interference y 0.5–1 mm several times the print error (± 0.1–0.2 mm), so it touches all the way round
Tip rounded a sharp edge tears

Point the tip toward the water or pressure side, so the pressure closes the lip against the wall instead of opening it.

Apply the rule from Layer orientation for mechanisms: the lip's length lies in the layer plane. A lip drawn as a flat wing that flexes in Z is stance A and works; its thickness comes out in whole layers. A flap whose length rises in Z is stance C: in a soft TPU it holds up worse and comes out with a stepped edge; in a semi-rigid one it snaps along a layer line. Prefer A. A flat wing needs something underneath while it prints: the natural choice is to have it grow from the part's first layers, on the bed, or to print the lip separately and flat.

It has three limits: pressure from the other side lifts it; grit gets under it; and if it spends time bent and hot, it stays deformed, which is the compression set from earlier. Against pressure, use the gasket in a groove with a stop, or an O-ring. Boots and bellows that protect moving shafts are a different problem, covered in Accordion bellows.

When it fails

Symptom, cause and fix
Symptom Cause Fix
Leak halfway between two screws the lid rim opens like a loaded beam a skirt or rib on the rim, or a narrower contact, before more screws
Leak at a corner bow plus opening δ exceed the squeeze measure the bow, raise h, fix the warp, put a screw near the corner
Water gets in next to a screw the hole is inside the gasket loop screws outside the gasket, gasket round each screw, or a blind boss
The gasket spills out by the screws and the lid rocks no compression stop a stop rim or limiters at each screw
The lid will not close with the gasket fitted the groove is too full fill ≤ ~85 % (Designing flexible parts)
Sealed when new, leaks after a few weeks or one hot day compression set: the TPU no longer recovers its squeeze a softer grade, more squeeze margin, or an O-ring if it runs hot
Leak across the gasket's width textured bed face or top lines crossing the gasket smooth plate, concentric pattern, or gasket printed onto the part
Water gets in far from the gasket the wall is porous, not the gasket Watertight printed parts
The lip lets through splashes coming from inside the pressure arrives on the side that opens it turn the tip toward the water side

How to test it

Force coupon, ten minutes. Print a length of the gasket section, put it between two flat plates on a scale and compress it to the design squeeze with a screw, using stacked feeler gauges as a stop. Pick the length so the load fits on the scale: 50 mm of an 85A bead gives about 50 N, about 5 kg, which fits on a kitchen scale; the solid 95A strip needs 10–20 mm and a bathroom scale. Convert the reading to newtons (1 kg ≈ 9.8 N) and divide by the coupon length: that is q. With that q, work out the pitch. The screw-and-scale setup is in Testing a mechanism before you trust it.

Contact. Close the box with strips of paper across the gasket at several points, including mid-span: all of them must stay trapped. Or coat the gasket with chalk or marker, close it and check that the print on the opposite face is continuous.

Water. Put a dry paper tissue inside and spray the box for a few minutes with the shower or a hose from every side. The stain on the tissue tells you where it got in: along the gasket line or through the wall. If it came through the wall, the fix lies in the wall, not in the gasket (Watertight printed parts). Real immersion is another matter: the pressure of a meter of water lifts a lip and calls for a gasket in a groove with a stop, or an O-ring.

Time. Leave it closed for 48 hours, plus a day somewhere hot if it will live outdoors; open it and repeat the water test. Compression set shows up here, not on day one. Call the gasket good when the tissue comes out dry after the spray and is still dry after the 48 hours.

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?