A 250 g device slides off the desk and lands on a tiled floor. With a solid printed bumper, the impact has almost no travel to spread over and reaches the electronics in full; a thin TPU pad crushes all the way and the device bottoms out with a clack. What protects is a low, steady force over enough travel, and a lattice that crushes at a chosen stress through nearly all of its thickness gives you that. The thickness comes from the drop height and the deceleration you can accept; the density and the area, from the mass.

The three zones of the crush curve

Compress a block of lattice and plot stress against strain, and three zones appear:

  1. Elastic region. A short climb: the cell walls bend.
  2. Plateau. The walls buckle (TPU), yield (ductile rigid plastic) or fracture (brittle rigid plastic) row by row, at an almost constant stress: the plateau stress σp.
  3. Densification. Beyond the densification strain εD, the walls touch and the stress climbs toward that of the solid material.
εDStressStrainUseful energyElasticPlateauIdealDensificationStressStrainTPU latticeHysteresis (energy dissipated)Rigid (ductile)Permanent crushInitial peakColumn-type cells
Left: the area under the plateau up to εD is the useful energy; the dashed rectangle is the ideal absorber. Right: TPU gives part of the energy back and dissipates only the area of the hysteresis loop; the ductile rigid lattice stays crushed; column-type cells give an initial peak and then a sawtooth.

The plateau is what you are after. To absorb a given energy with the lowest possible peak force, the force has to stay constant over the longest possible travel. On a force-travel curve, the ideal absorber is a rectangle. The energy absorbed per unit volume is the area under the plateau up to εD: W ≈ σp·εD. Past εD, the pad behaves like a solid block and the whole impact goes through. It is the same area-under-the-curve criterion as in Stiffness, strength and toughness.

Gibson and Ashby relate the plateau to the relative density ρ*/ρ, the fraction of the volume that is material (Es: modulus of the solid material; σs: its strength):

Plateau and densification of a lattice (Gibson and Ashby)
Behavior Plateau stress σp Typical material
Elastic buckling ≈ 0.05·Es·(ρ*/ρ)² TPU
Plastic collapse ≈ 0.3·σs·(ρ*/ρ)^1.5 PETG, PA, PC
Brittle fracture ≈ 0.2·σs·(ρ*/ρ)^1.5 PLA
Densification εD ≈ 1 − 1.4·ρ*/ρ all

The elastic-buckling and densification laws are the same as in TPU and lattice springs. They hold up to ρ*/ρ ≈ 0.3. Printed cells stray from them: trust the exponents and get the coefficient from a coupon.

What that means in numbers: at 10 % density, εD ≈ 0.86; at 20 %, 0.72; at 30 %, 0.58. A denser pad is harder and also has less useful travel.

Sizing a pad: thickness and density

Energy. For a falling mass, E = m·g·h; for a moving mass, E = ½·m·v². A 250 g mass dropped from 1 m carries 2.45 J and hits the floor at v = √(2·g·h) = 4.4 m/s.

Thickness first. It does not depend on the material. With a flat plateau the force is constant, so the stopping distance is s = h/G, where G is the maximum acceptable deceleration in multiples of g (ignoring the small m·g·s term). The crush has to fit inside the plateau: T ≥ s/εD, and with a margin, T ≥ s/(0.8·εD). For 1 m and 100 g: s = 10 mm, and T ≈ 15–22 mm depending on density (10 to 30 %). If you can only accept half the G, the pad has to be twice as thick. That rules out thin pads: a 3 mm layer of TPU will not stop a 1 m drop gently, however soft or hard it is.

s = h/G assumes a perfectly flat plateau. A TPU lattice's plateau rises as it crushes, so the peak exceeds h/s: for a linear spring it reaches 2·h/s. Design with a margin.

Then density and area. The plateau has to deliver the force F = m·G·g over the contact area A: σp = m·G·g/A. Using your material's law, solve for ρ*/ρ and check it stays below 0.3. If it does not, enlarge the area or move to a harder TPU or a rigid lattice.

Thickness TεD·TTravelForceDevice limit m·G·gToo softRightToo hardPeak on contactBottoms out
Same pad, same energy (the three areas are equal), three densities. The soft one bottoms out with a peak at the end; the hard one stops in a few millimeters with a peak on contact; the right one uses the thickness without exceeding the device's limit.

If it is too soft, the plateau sits below the σp you need, the pad reaches εD with energy to spare and the force shoots up at the end. If it is too dense, it stops in a fraction of the thickness at a high force and the peak comes at the start. To the device, the two peaks feel much the same. Only the travel tells them apart, and travel is what the drop test measures.

How many g your device can take. This book cannot give you your device's fragility, the g it survives without damage. As an order of magnitude, rugged, well-secured electronics survive anywhere from a few tens of g to about 100 g; lenses, glass and a spinning hard drive survive less (switched off, the drive takes far more). If the manufacturer quotes a shock rating, use it with its pulse duration: the same device survives more g in a shorter pulse, and a pad's stop lasts a few milliseconds. With no data, 100 g is a working target, not a guarantee.

TPU or rigid: many knocks or one

TPU lattice. It buckles elastically, recovers and survives many impacts: bumpers, feet, knee and elbow pads, a drone's landing gear. It has three limits:

  • Rebound. Part of the energy is stored and given back, and the device bounces. Only the hysteresis loop is dissipated (Designing flexible parts); how much depends on the grade and the strain, and you can see it on the load-unload curve. So a TPU pad stops less than its travel suggests: measure the rebound.
  • Time. Under a sustained load, TPU creeps and does not recover its height (Creep and fatigue).
  • Modulus. It changes with temperature and from brand to brand: Bambu Lab's datasheet for its TPU 95A gives about 9.2 MPa in XY, and some other 95A filaments are several times stiffer.

Its plateau is low, so TPU lattices suit light masses or large areas. Foaming TPU is another way to lower the plateau without changing the geometry (TPU and flexible filaments).

Rigid lattice (PLA, PETG, PA, PC). At the same density its plateau is tens of times higher, so it absorbs far more energy per gram. But it stays crushed: it is single-use, like the expanded polystyrene in a helmet or a car's crumple zone. PLA fails in a brittle way: it gives a sawtooth plateau and sheds fragments. PETG, PA and PC fold more evenly. Use it in parts you replace after the impact: the crash block on a drone or RC car chassis, the nose of a model rocket, a packing block for shipping.

At impact speeds plastics are stiffer: a plateau measured slowly in a press underestimates the one in the impact, by a ratio that depends on the cell. In TPU, higher speed also raises the initial peak and brings densification forward. Leave a margin on thickness and confirm with a drop test, never with the press alone.

Which cell: a flat plateau and no initial peak

Bending-dominated cells (the gyroid and other TPMS, BCC and foam-like 3D infills) give a smooth, flat plateau: they are the best absorbers. Stretch-dominated cells are stiffer per gram but buckle all at once: a high initial peak, a drop and then a sawtooth. This group includes the octet cell and the 2D infills whose walls are vertical columns loaded in Z: grid, honeycomb, triangles. That peak is what breaks the device. The difference between the two families is covered in Auxetics and lattices.

Column-type cells are not banned. Honeycomb loaded along the axis of its cells is the classic industrial absorber because it gives a lot of energy per gram, but it is used pre-crushed or with a collapse initiator. Do the same: a chamfer or a thinner first row, so the collapse starts at one end rather than everywhere at once.

Walls and solid layers are columns too. The walls and the top and bottom layers around the infill form a stiff shell that carries the load for the first few millimeters and creates the initial peak. In a crash pad, leave the impact face open (no top layers) and use 1–2 walls, or model the lattice open. In a TPU foot, on the other hand, 2 walls is the right call (Designing flexible parts).

If you do not know the drop height, grade the density: a soft layer takes the light knocks, a denser one the hard ones. The resulting progressive curve is covered in TPU and lattice springs.

The cheapest way to make it is the slicer's infill (gyroid or, in OrcaSlicer as of late 2026, TPMS-D and TPMS-FK) with a density modifier per region (Modifiers by region and height, Walls, perimeters and infill). Model the cells when the lattice will be visible, has to let air through, follow a surface or be graded in one direction.

Printing it so it crushes properly

Orientation. TPU hardly cares (Bambu Lab's TPU 95A datasheet gives a modulus of 7.8 MPa in Z against 9.2 in XY): orient it with overhangs in mind. For design, a rigid block is half as strong in Z as in XY (Layer adhesion and anisotropy), but that weakness is in tension. Compressed in Z, perpendicular to the layers, the lattice squeezes its layers together. Loaded in the plane of the layers (in XY), it spreads sideways as it crushes and can delaminate along the layer bonds instead of crushing cell by cell. So make the impact arrive in Z on a rigid block, and check it with the coupon. The gyroid is nearly isotropic as a geometry, not as a printed part.

Minimum thickness. With a 0.4 mm nozzle, a two-line wall measures 0.9 mm and is the minimum; a functional part gets three lines, 1.2 mm. The same goes for struts. In TPU, self-supporting cells with no horizontal bridges (TPU and lattice springs).

Dry the TPU before printing (TPU and flexible filaments). Wet TPU gives porous, weak walls and a lower, more scattered plateau.

Worked example: a pad for a 250 g device

The brief: protect a 250 g handheld device against a flat 1 m drop onto tiles, many times, in TPU 95A, with a peak of no more than 100 g. The resting face measures 60 × 40 mm, so the pad covers 2400 mm².

Step 1, energy. E = 0.25 · 9.81 · 1.0 = 2.45 J.

Step 2, travel. s = h/G = 1000/100 = 10 mm.

Step 3, plateau. F = 0.25 · 100 · 9.81 = 245 N, so σp = 245/2400 = 0.10 MPa.

Step 4, density. ρ*/ρ = √(σp/(0.05·Es)). With Bambu Lab's TPU 95A at 9 MPa you get 0.47, outside the model: that TPU is too soft for this mass on this area. You have three options: more area, a harder TPU, or a lower G and a thicker pad. The example goes on with a stiffer 95A of Es ≈ 26 MPa (an example value: check your filament's datasheet): √(0.10/1.3) = 0.28, and εD ≈ 0.61. The formula gives the starting point; the coupon sets the value.

Step 5, thickness. T = s/(0.8·εD) = 10/(0.8 · 0.61) ≈ 20 mm. Energy check: σp·εD·A·T ≈ 0.10 · 0.61 · 2400 · 20 ≈ 2.9 J ≥ 2.45 J. It passes, with some margin.

Step 6, coupon. Print three 20 × 20 × 20 mm gyroid blocks: one at the chosen infill and two at 5 percentage points above and below, all without a top layer on the loaded face and with the same walls as the part (Test coupons). With a 400 mm² face, the plateau calls for about 40 N, around 4 kg: within reach of the kitchen scale in the screw-and-scale rig (Testing a mechanism before you trust it).

Load them slowly and read the force where the curve flattens: σp = F/400 mm². A small coupon carries proportionally more wall than the pad, so it comes out a little harder: allow for that when you read it.

Suppose the middle block reads 0.085 MPa (a made-up reading for the example). Since the elastic-buckling plateau goes with the square of density, multiply the density by √(0.10/0.085) = 1.08: you go from 0.28 to 0.30, right at the edge of the model. Raising the density lowers εD, to about 0.58, so recompute the thickness: T = 10/(0.8 · 0.58) ≈ 22 mm. Print one more block to confirm. If the correction took you above 0.3, the way out is more area or a harder TPU, not more density.

Step 7, drop test with a dummy of the same mass (see "How to test it", below).

The rigid alternative. The same brief in PLA gyroid at 10 % (σs ≈ 35 MPa in tension in XY): σp ≈ 0.2 · 35 · 0.10^1.5 ≈ 0.22 MPa. For the same 245 N, about 1100 mm² is enough, and with εD ≈ 0.86 the thickness drops to about 15 mm. The brittle law calls for flexural strength, which is higher than tensile, so the real plateau will come out higher and so will the peak: size the area from the plateau measured on the coupon, not from this number. And it crushes only once: it suits a part you replace, not everyday knocks.

When it fails

Symptom, cause and fix
Symptom Cause Fix
The device breaks and the pad barely crushes Too dense (high plateau), or the walls and solid layers carry the impact Lower the density, open the impact face or reduce the contact area (σp·A must equal m·G·g, no more); if it then bottoms out, make it thicker
Loud clack and a fully crushed pad Bottoming out: the energy exceeds σp·εD·volume Make the pad thicker; denser only if the plateau sits below the σp you need
A hard jolt on first contact, then soft Column-type cell (2D infill loaded in Z) or walls giving an initial peak Switch to gyroid or TPMS, add an initiator row, remove walls
The device bounces hard The TPU stores the energy and gives it back Lower plateau with more travel, softer or foaming TPU; or a single-use rigid insert
The rigid block delaminates Loaded in XY, in the plane of the layers Make the impact arrive in Z; use a ductile material
The TPU pad has lost height after weeks under the device Compression set Do not let it carry weight at rest or, if it has to, lower the stress (Creep and fatigue)
Much softer or harder than calculated Infill % is not ρ*/ρ; modulus varies by brand; wet TPU Weigh the part, print a coupon, dry the filament
Harder in winter TPU stiffens in the cold Test at the temperature of use

How to test it

In a press, slowly. The coupon from step 6 gives σp and εD. εD is where the curve starts climbing again.

Drop. Print a box and ballast it with sand, coins or modeling clay up to the device's mass, fit the pad and drop it five times from the design height onto the real floor. Film it in slow motion (240 fps, which many phones offer) with a ruler beside it, and measure the crush s in the lowest frame. At 10 mm and 4.4 m/s the stop lasts about 4–5 ms: you will see one or two frames, and they rarely land exactly at the bottom, so the crush you see is less than the real one. Keep the largest crush of the five drops. h/s gives the mean deceleration (1000 mm / 10 mm = 100 g); the real peak lies between h/s, for a flat plateau, and 2·h/s, for a linear spring.

  • If s approaches T·εD, you are bottoming out.
  • If s stays at a few millimeters in a 20 mm pad, it is too hard.
  • Phone accelerometer apps saturate well below 100 g: they cannot measure the peak.

As a witness, put a sheet of modeling clay under the sensitive point of the dummy: if it is marked, the impact got through.

After the drops, measure the pad's height again: in TPU it tells you how much it has not recovered; in rigid plastic, how much it has crushed. In TPU, measure again after 48 h (Testing a mechanism before you trust it).

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?