kapy academy

Crush ribs and compliant pins

20 min readUpdated Nov 2026

A cylindrical press fit wants 0.05–0.10 mm of interference on the diameter, measured from the zero of your coupon, and a well-calibrated printer wanders ±0.05–0.15 mm on that same diameter. In three cases that scatter is as large as the interference: diameters above about 10 mm, horizontal holes and small PLA pins. The same file comes out loose one day and splits the boss the next. The fix is a different joint: a small feature designed to yield takes up the interference, and a 0.1 mm error shifts the force a little instead of multiplying it.

Why a plain cylinder is unforgiving and a rib is not

In a plain cylinder the spring is the whole wall. The force is the hoop stiffness of the ring times the interference δ on the diameter, and that stiffness is high, so the useful band of δ is a few hundredths of a millimeter wide. Below it nothing holds; above it the hole strain, δ/D, goes past the material's limit. Draw δ = 0.05 with a scatter of ±0.05 and the real δ runs from 0 to 0.10 mm: from 0 to 200 % of the intended force. On a Ø5 PLA pin that is 0 to 2.0 % strain, beyond the 1–1.5 % a permanent joint will take.

Crush ribs are narrow ribs inside the hole that yield plastically on assembly, and only their crests touch. The first time the part goes in, each crest yields locally, and the force is set by the width of the contact band, not by the stiffness of a whole ring. On a narrow, rounded rib that width changes little with how much is crushed: an extra 0.1 mm of interference raises the force by 20–35 %, it does not double it. The wall sees a few point loads, which it handles well, instead of straining as a ring, and it does not split.

A compliant pin has a slot, and its legs flex inside the hole: they form a spring whose working deflection is several times the scatter. The force is the legs' stiffness times their deflection y. If each leg closes y = 0.15 mm, a scatter of ±0.05 on the diameter (±0.025 per leg) moves the force by ±17 %, and one of ±0.1 by ±33 %: it keeps holding across the whole range, instead of going from 0 to 200 %. The bending is elastic, so unlike the ribs, the pin comes out and goes back in.

Crush ribs come from injection molding, and the compliant pin from the eye-of-the-needle pin in circuit-board connectors. The interference figure for a plain cylinder, the δ/D table and the coupon zero are in Choosing the fit: clearance, transition, interference.

the boss splitsprinter scatterprinter scatter−0.100.10.20.30.4actual interference on the diameter (mm)relative holding forceplain cylindercrush ribscompliant pinforce variation
The same printer scatter, three joints. The plain cylinder goes from not holding to splitting the boss; the ribs climb gently once crushed and the compliant pin follows a shallow straight line.

Rib geometry

Put them in the hole of the printed part when what goes in is a hard, bought part: a bearing, a magnet, a steel dowel, a hex bit, a pen refill. Put them on the outside of a printed boss when the hole is in something you cannot change, such as a drilled hole in wood or sheet metal. Between two printed parts, put them on whichever part prints in the better orientation.

Every dimension starts from your zero: the step of the clearance coupon at which the real part goes in by hand with no play, printed in the final material and orientation (Test coupons). The hole you draw is not the hole you print, for the reasons in Why holes print small; the zero already accounts for that. The figures in this table are starting points to test, not a standard: there is none for printed ribs. They come from molding practice (at least three ribs, about 0.25 mm of interference) and from the printing community's experience (start at 0.2–0.3 mm and print a coupon).

Crush ribs: starting point (from your coupon zero)
Dimension Value Why
Bore between ribs zero + 0.2 mm on the diameter (0.1 per side) the wall never touches the part, even when the hole prints small
Crest circle zero − 0.2 to − 0.4 mm on the diameter; − 0.3 to start 0.1–0.2 mm of crush per side, two to three times the per-side scatter
Rib height above the bore 0.2–0.3 mm; 0.25 half the difference between bore and crests
Base width 0.8–1.2 mm, rounded crest 2–3 line widths with a 0.4 nozzle
Count 3 up to ~10 mm; 4–6 from 10 to 25 mm; 6–8 in a bearing seat evenly spaced
Lead-in ramp ≥ 1 mm along the axis crushing starts gradually
Wall behind ≥ 1.2 mm (3 lines) for a magnet or bit; 2–3 mm for a bearing walls, not infill

Mixing up diameter and radius is the costliest mistake here. The arithmetic, once: a crest circle at zero − 0.3 on the diameter crushes 0.15 mm per side, on each rib. The bore at zero + 0.2 leaves 0.1 mm of air per side. The rib height is half the difference between the two diameters: (0.2 + 0.3) / 2 = 0.25 mm.

A rib narrower than one line width will not print: the slicer drops it. One much wider, from about 1.5 mm as a guide, crushes poorly and behaves like a piece of plain cylinder. The rib is a bump in the wall's outer bead, so the slicer traces it with that bead; it is not a separate island. At 1 mm wide and 0.25 high it is a low bump, not a blade: that is why the crest is rounded and why the force grows little with crush.

Three ribs are enough up to about 10 mm: three contacts define a circle and center the part on their own. On larger diameters more ribs share the load; in a bearing they also support the ring at more points and ovalise it less. Odd or even, they center equally well; what matters is that they are evenly spaced.

The ramp rises 0.25 mm over at least 1 mm of height and prints cleanly. If the part goes in from the bed face, keep the 0.5 × 45° chamfer at the mouth against elephant's foot; better still, insert it from the top face. The crushed material piles up at the bottom of the ribs: in a blind hole leave 0.5–1 mm of free depth below the part, as the blind-hole rule in Press fits that do not crack asks.

The wall behind needs less than the boss of a plain fit, because the force is capped by the ribs yielding. Even so, the point loads flex the ring between one rib and the next: build it from walls, not infill.

Two warnings about the slicer. Ribs are 0.25 mm details: export at a high enough resolution (STL, 3MF or STEP for the slicer). And the XY hole compensation in slicers as of late 2026 moves the ribs along with the bore: take your zero with the same print settings.

bearing ringwallborezero + 0.2crest circlezero − 0.3on the diameterairbase 0.8–1.2height 0.25crushed crestbearing ringentryramp ≥ 1 mmlayersfree depth 0.5–1crushed materialwall
Six ribs in a 608 seat. The ring touches only the crests and stands clear of the wall. In section, each rib is a strip running in Z with a lead-in ramp, and the crushed material needs room at the bottom.

Rib orientation and material

With the hole axis vertical, which is the usual case, the ribs run in Z: every layer carries its bump and the crush is a radial compression within the layer. Nothing pulls the layers apart, and the wall does not get the hoop strain that opens a plain cylinder along its seam.

With the axis horizontal, the roof of the hole sags: in 6 to 10 mm holes it drops 0.1–0.3 mm, and a rib at the crown prints inside that sag. Put one at the bottom and two at 60° from the crown, one either side, none at the top; above 10 mm, make the roof a teardrop or a flat. If you have to press something into a horizontal hole, ribs are the way to do it; a plain cylinder there is a lottery.

On a printed boss the ribs run along its axis with the same figures and the sign flipped: crests at zero + 0.3 and core at zero − 0.2, with the zero taken in the real hole. The boss prints best standing up or lying on flat faces.

The material has to deform, not chip. PETG, PA and ABS/ASA crush cleanly. PLA will do for light parts, but its crest can flake instead of flattening, and the flakes stay loose in the hole. TPU does not work for ribs: it does not crush, it springs back and behaves like an O-ring. Fiber-filled materials are brittle at the crest and do not work either. The choice by mechanism is in Which plastic for which mechanism.

A crushed rib also relaxes: its contact pressure falls over the days, as in any press fit. It holds better than a plain cylinder because it starts from a plastically yielded, repeatable state, not because it is free of creep. Under sustained load or heat, the crests keep flattening. For ribs under sustained load, use PC or ASA; PLA and PETG are fine for a light load with no heat (Creep and fatigue). Under load, an unfilled part works up to about 15–20 °C below its HDT at 0.45 MPa: PLA about 40 °C, PETG 50, ASA 80–85 (Heat, cold, sunlight and chemicals).

Crush ribs work once. The second insertion is looser because the crests are already flat. If the part has to come apart, use a compliant pin or flex fins, blades leaning 30–45° off the radius that the interference bends within the layer plane and that are sized as a cantilever (Print-friendly snap fits).

Worked example: a ribbed seat for a 608 bearing

The brief: a 608 (Ø22 × 7) in a PETG part, permanent, with a light radial load and the housing printed standing up. The bearing's dimensions and shoulders are in Standard bearings and bushings; which ring takes the interference and which one you must not squeeze, in Seating bearings and bushings.

  1. The zero. Print the clearance coupon around Ø22, in PETG and standing up. The step at which the bearing goes in by hand with no play is your zero C; say C = 22.15 as drawn.
  2. The bore. C + 0.2 = 22.35 as drawn. The ring never touches the wall.
  3. The ribs. Six, every 60°. Crest circle C − 0.3 = 21.85; height (22.35 − 21.85) / 2 = 0.25 mm; 1.0 mm base, rounded crest, 1 mm ramp at the mouth, at the top.
  4. The scatter. If the hole prints 0.1 mm larger or smaller on the diameter, each rib crushes 0.1 or 0.2 mm per side instead of 0.15: it still crushes, it never goes loose, and no solid ring squeezes the bearing race. Compare a plain seat drawn at C − 0.05 (0.05 of interference): with the same ±0.1 scatter it runs from 0.05 of clearance to 0.15 of interference against a steel ring.
  5. The force. With 0.15 crushed, each rib's contact band is about 0.7–0.9 mm wide along the 7 mm of the ring. With a yield pressure of the order of 50 MPa for PETG, that is about 250–300 N radially per rib, about 1500–1800 N in all, and with μ ≈ 0.25 (printed plastic on steel) about 400 N to push it in. It is an order of magnitude, but it explains why you fit it with a press or a vice, not your thumb.
  6. The wall. 3 mm of wall behind the ribs and, at the bottom, a 1 mm tall shoulder with a Ø19.5–20 through-opening (not exceeding SKF's Da max of 20 mm) that supports only the outer ring. The bearing bottoms on the shoulder; the ribs only hold it radially.
  7. Assembly. From the top face, square, with a vice or a socket bearing on the outer ring. Never push on the inner ring.
  8. Retention. If it has to last for years or it vibrates, add a printed cap or a drop of adhesive on the outer ring: the ribs center, the cap or the adhesive retains. Under heavy radial load or shock the ribs keep flattening; this is no longer the right joint. Use a shoulder and cap, or a metal housing.

Compliant pins: a slotted pin that closes up

A compliant pin is a pin with an axial slot and no nub. A snap pin is two cantilevers: its slot, root and orientation are sized in Split pins and spring clips, and the compliant pin takes them from there. What changes is how it holds. The shank is a sliding fit: zero − 0.4 on the diameter, 0.20 mm per side on a modern bedslinger (Real printed clearances). Only a short bulge, 1.5–2 mm long and near the tips of the legs, is larger than the hole. Going in, the bulge forces each leg to close by a deflection y; the rest of the shank keeps its clearance. It holds by the elastic push of the legs times the friction coefficient, so it works in a blind hole too.

The bulge sets the deflection. Draw it at zero + 0.3 mm on the diameter (try 0.2 to 0.4), which is y = 0.15 mm per leg. With a scatter of ±0.1 on the diameter that is three times the per-side scatter, and the force does not depend on how the print comes out. If your machine scatters ±0.15, raise the bulge to + 0.4 and lengthen the slot to stay within the strain budget. The strain at the root is the snap pin's, with t the leg thickness and L the slot length up to the bulge. In repeated use PLA takes 1–1.5 % strain (1 % if it opens daily) and PETG 2 % (Print-friendly snap fits). The slot and its bottom are the snap pin's.

The force from each leg is P = 3·E·I·y/L³ (load at the tip). The normal force on the wall is 2P, and the pull-out force is of the order of μ·2P, with μ = 0.3–0.5 between printed plastics. The grip is modest on purpose. If you need more, use more pins or add a nub.

There is a closed variant, the eye-of-the-needle: the slot sits in the middle of the pin, with a solid tip, and the bulge at the center of the slot. Each leg works as a fixed-fixed beam loaded at the center, and ε ≈ 12·t·y/L², with L the full slot length. The formula is derived, not measured (two cantilevers of L/2 with a guided end): treat it as a starting point. At the same L the strain is 8 times higher and the stiffness 64 times higher than with an open slot. For the same strain it needs a slot about 2.8 times longer and still comes out about 2.8 times stiffer: more force and better centering. The solid tip survives knocks in handling and prints as a single closed contour.

It is oriented like the snap pin, lying down with the slot vertical (Split pins and spring clips).

The legs stay flexed inside the hole, so their push relaxes over the days. Design the grip with the deflection it already has and measure it at 48 h. If it is not enough by then, add pins or a nub, not more interference: a bigger bulge only pushes the root closer to its limit.

Two slotted Ø5 pins from the front, in a hole through two 4 mm plates. Left, open slot: its two cantilevered legs close inside the hole and the bulge near the tip pushes on the wall. Right, eye of the needle: the 22.4 mm slot sits in the middle of the pin, with a solid tip, and its two beams bow inwards at the middle. Both are pulled out until the bulge leaves the hole, the legs spring back straight, and they are pushed back in
Open slot: cantilever legs with the bulge at the tip. Closed slot: fixed-fixed beams with a solid tip. Both print lying on a flat with the slot vertical, so the legs flex in the plane of the layer. The bulge is drawn twice its size (0.3 a side) and the slot wider, so the legs can be seen closing; each leg is a rigid segment turning 0.15·L from the root, and each beam two halves hinged in the middle.

Worked example: a Ø5 slotted pin in a printed hole

The brief: join two PLA plates with a Ø5 pin, also in PLA, that goes in by hand and can be pulled out several times. The holes print vertical and the measured zero is 5.0.

  1. Dimensions. Shank Ø4.6 (sliding). Bulge Ø5.3 (zero + 0.3), so y = 0.15 per leg. Slot s = 2·0.15 + 0.3 = 0.6 mm. Flats 3.6 mm apart (width w). Each leg bends across the shank diameter, so its thickness comes from that diameter: t = (4.6 − 0.6) / 2 = 2.0 mm.
  2. Slot length. In PLA, with ε = 1 %: L ≥ √(1.5·2.0·0.15 / 0.01) ≈ 6.7 mm, about 7.2 with the section margin; take L = 8 mm. Check: 1.5·2.0·0.15 / 64 ≈ 0.70 %, around 0.8 % with the real section. In PETG, with ε = 2 %: L ≥ 4.7 mm, about 5.1 with the margin; round up to 6 mm.
  3. Force. With the real section of each leg (half a Ø4.6 circle minus half the slot, trimmed by the flats), I ≈ 1.75 mm⁴; the rectangle w·t³/12 would give 2.4. With PLA's design E of 2.5 GPa, P = 3·2500·1.75·0.15 / 8³ ≈ 3.8 N per leg, about 7.7 N on the wall. Pull-out ≈ 0.4·7.7 ≈ 3 N. To push it in, with a 30° lead-in cone and μ = 0.4, the wedge gives W = 2P·(μ + tan 30°) / (1 − μ·tan 30°) ≈ 10 N. It is an order of magnitude: the real figure comes from measuring.
  4. Scatter. ±0.05 mm on the bulge diameter moves y by ±0.025: the force varies by ±17 %; with ±0.1, by ±33 %. The same joint as a plain cylinder, with 0.05 of interference and the same scatter, would run from not holding to 2.0 % strain, beyond PLA's permanent limit.
  5. Printing. Lying on a flat, slot vertical. A 25–35° lead-in cone ahead of the bulge, the same angle as on the snap pin, and a 0.5 × 45° chamfer on the edge that sits on the bed.
  6. If 3 N is not enough. Use two pins, move to PETG with a shorter, stiffer leg (more force within the same strain budget) or switch to the snap pin with a nub.

When it fails

Symptom → cause → fix
Symptom Cause Fix
Loose even though the ribs are modeled Crest circle taken from nominal, not from the zero; ribs narrower than a line width, dropped by the slicer Coupon zero; base ≥ 0.8 mm; check the slicer preview
The boss splits along the seam on assembly The bore touches the part (drawn at zero or below); ribs too wide to crush Bore at zero + 0.2; base ≤ 1.2 mm
The part goes in crooked or does not bottom out Ribs without a ramp; crushed material with no room in a blind hole 1 mm ramp, 0.5–1 mm free depth, insert from the top face
Tight the first time, loose the second Crush ribs work once Flex fins or a compliant pin if it has to come apart
PLA ribs shed flakes and hold poorly The PLA crest chips instead of deforming PETG, PA or ABS/ASA
The bearing works loose under load The ribs keep flattening under radial load or heat Shoulder and cap, or a different seat
The pin legs snap at the root Printed standing up (stance C); ε over the limit (short slot, PLA fitted many times); sharp corner at the bottom Lying on a flat, longer slot, rounded bottom, PETG
The pin will not go in Slot too narrow (the legs touch before reaching deflection y); elephant's foot on the bulge s ≥ 2y + 0.3; chamfer on the bed edge; lead-in cone
Holds on day one, wobbles weeks later The flexed legs relax; heat Measure at 48 h and design to that figure; more pins or a nub, not more interference

How to test it

For the ribs, print a coupon with the real bore and three crest circles (zero − 0.2, − 0.3 and − 0.4), in the final material and orientation. Push the real part in. Look for whitening in the wall behind the ribs and at the mouth. After 48 h, measure the pull-out force with a spring balance; if there is nothing to grip, push it out from behind through a small hole. Keep the smallest crush that holds with margin.

For the compliant pin, print a coupon with three bulges (zero + 0.2, + 0.3 and + 0.4) on the real slot length. Fit and remove each pin ten times, and measure the pull-out force on the first and the tenth. Look at the slot root under raking light: whitening warns you before the crack does.

If the part works warm, run the hot test at the service temperature under load: 40 °C for PLA and 50 °C for PETG. The rig and the method are in Testing a mechanism before you trust it.

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?