kapy academy

Which plastic for which mechanism

15 min readUpdated Nov 2026

A mechanism asks a plastic three questions: how far can it bend and come back (the allowable strain), how hard does it push back (the modulus), and does it keep pushing over time and in the heat (creep and relaxation). No plastic wins all three: the PLA clip on a lid breaks on the 300th opening, the same file in PETG survives but closes with a soft click, and a PETG latch that spends the summer shut stops gripping. Pick the material from the job the part does in the mechanism, not from a property list.

Bend, push, hold

How far does it bend without breaking, again and again? Every cycle grows a crack from a notch: the valley between two layers, the seam, a root with no fillet. The smaller the strain amplitude, the more cycles it lasts. For repeated use the limits are: PLA 1–1.5 % (1 % if the part opens daily), ABS/ASA 1.5 %, PETG 2 %, PC 2 %, conditioned PA 4 % and PP 6 %. Fiber-filled filaments sit below PLA. These figures come from Print-friendly snap fits, and the fatigue mechanism is covered in Creep and fatigue.

How hard does it push? With the same geometry and the same deflection, force is proportional to the modulus E. The design moduli, flexural in XY and reduced for a printed part, are: PLA 2.5 GPa, PC 2.1, ABS and ASA 1.7, PETG 1.6, PA 1.0 conditioned, stiffer when dry, and PP 0.45 (it varies with grade). TPU 95A is around 9 MPa (0.009 GPa). Swap PLA for PETG in the same file and the click loses more than a third of its force. The difference between stiffness and strength is in Stiffness, strength and toughness.

Does it keep that up over time and in the heat? Under a fixed load, the part keeps deforming: that is creep. Held at a fixed position, it loses force: that is relaxation. In a mechanism, a clip, latch or detent that spends its time deflected loses its preload, and loses it faster when warm.

Here is the conflict: the plastics that bend furthest (PP, PA, TPU) push the least and creep the most, and the stiff ones (PLA, fiber-filled filaments) bend the least.

Creep and heat

At room temperature, PLA holds a light sustained load about as well as PETG: no reliable data on printed parts says which creeps more. PETG only wins when the part gets warm. For a sustained load, use PC or ASA, or a fiber-filled filament if the part is not a spring (Creep and fatigue).

Ranked for sustained load at room temperature, best to worst: unfilled PC; ABS and ASA; PLA ≈ PETG/PCTG; unfilled PA, worse when wet; PP, which lets a hook slowly open; and TPU, which carries no load. Fiber-filled filaments are the best along the bead, but between layers the matrix decides.

Under load, an unfilled part works up to about 15–20 °C below its HDT at 0.45 MPa: PLA about 40 °C, PETG 50, ABS 70, ASA 80, PC 95 (Heat, cold, sunlight and chemicals).

In summer, a car's dashboard in the sun reaches 70–100 °C. A loaded part there needs a fiber-filled compound: PA-CF, PET-CF or PPA-CF. Unloaded or in the shade, in the console or the glovebox, ASA, PC or annealed PLA-HT will do, and PC wherever it takes knocks. Inside a car, never PLA or PETG.

The part's job picks the plastic

Start from what the part does, not from the filament loaded in the printer.

diagram
The part's job decides the plastic. Any change of material means recalibrating the fits.
Job in the mechanism → plastic
Job First choice Also works Avoid Why
Clip assembled once any rigid plastic PLA up to 2 % assembly strain, PETG and PC up to 3–4 % fiber-filled filaments, unless the assembly strain stays below PLA's it only flexes once: the assembly limit applies, not the repeated-use one
Clip opened often PETG/PCTG, PC PA; PLA only at ≤ 1 % fiber-filled filaments cycles × amplitude: PETG's 2 % doubles PLA's margin
180° living hinge PP TPU PLA, PETG, ABS PP up to ~10⁶ cycles, TPU > 2 × 10⁶; the rest, < 1000
Flexure (small angle, many cycles) PETG, PC, PA PLA with a long blade at ≤ 1 % fiber-filled filaments the length follows from the allowable strain
Spring that must keep its force bought steel spring PC or PETG, if the spring only works during the gesture and rests unloaded between uses PLA, except for a prototype relaxation eats the preload
Clamp or preload for months PC, ASA, fiber-filled filament PLA and PETG when cool and lightly loaded PP and TPU if they carry the load creep and relaxation
Sliding and meshing PA, PA-CF, POM, low-friction filament — PETG on PETG, PLA on PLA it binds, squeaks and wears
Soft contact, seals, grip TPU 95A–85A — any rigid plastic absorbs and recovers
Hot environment ASA, PC, PA-CF/PET-CF — PLA, PETG service temperature under load, in "Creep and heat"

Some rows need more detail. Permanent and reversible clips are told apart in Snap-fit catches. Living-hinge bands are 0.4–0.6 mm thick, with the beads perpendicular to the fold; the rest of the design is in Living hinges and flexures. To size a flexure blade, follow Sizing a flexure as a pivot. For a spring that has to keep its force, the sensible choice is steel (Using bought steel springs); soft, long-travel springs have their own article in TPU and lattice springs. For sliding, always pair different materials: coefficients and lubricants are in Friction and wear, and tooth strength in Sizing a gear that holds. Heat and UV are covered in Heat, cold, sunlight and chemicals.

Worked example: the same clip in six plastics

A box lid that opens daily has a cantilever snap-fit clip with a 1.0 mm undercut, which is the deflection y the arm takes on assembly, thickness t = 1.5 mm and width w = 6 mm, printed flat (stance A in Layer orientation for mechanisms). For each material, work out the shortest arm that respects its repeated-use strain, and the force it gives with its design modulus:

L = √(1.5 · t · y / ε) and P = w · E · t² · ε / (6 L), with L ≥ 5t = 7.5 mm.

Clip with y 1.0 · t 1.5 · w 6 mm, sized to each material's repeated-use limit
Material Design ε E (GPa) Arm L Force at the undercut
PLA 1 % 2.5 15.0 mm ≈ 3.8 N
ABS / ASA 1.5 % 1.7 12.2 mm ≈ 4.7 N
PETG 2 % 1.6 10.6 mm ≈ 6.8 N
PC 2 % 2.1 10.6 mm ≈ 8.9 N
PA 4 % 1.0 conditioned (more when dry) 7.5 mm (5t minimum) ≈ 12 N conditioned, more when dry
PP 4 % (of its 6 %) 0.45 (it varies with grade) 7.5 mm (5t minimum) ≈ 5.4 N, by grade
Arm lengthClick forcePLA · 15.0 mm · 3.8 NABS/ASA · 12.2 mm · 4.7 NPETG · 10.6 mm · 6.8 NPC · 10.6 mm · 8.9 NPA · 7.5 mmDepends on moisturePP · 7.5 mm · ≈5 NDepends on gradeMinimum L ≥ 5t = 7.5 mmy 1.0 mm · t 1.5 mm · w 6 mm · repeated-use strain
Each plastic sized to its own repeated-use strain: PLA, the stiffest, needs the longest arm and gives the softest click.

First reading. When each plastic works at its own limit, the one that takes more strain gets the shorter arm. The arm shortens with the square root of ε and stiffness rises with 1/L³, so PETG and PC, despite a lower modulus than PLA, more than make up for it with a shorter arm and close more firmly. The PLA clip is the longest and the softest: the intuition that PLA, being stiffer, makes stronger clips breaks down when the clip opens often. PP and PA hit the 5t minimum. PA, with its design modulus, gives the firmest click in the table; PP, at 0.45 GPa, pushes less than PETG. They are the least reliable figures: PP's changes with the grade and PA's with the day's humidity. Measure the force before you count on it.

Second reading: same file, different material. PLA's 15 mm arm printed in PETG works at 1 % of its 2 %, with twice the margin, but pushes with 1.6/2.5 ≈ 64 % of the force: about 2.4 N. That is the clip from the opening paragraph: it survives, but closes soft. If you want PETG's life with PLA's click, shorten the arm. At 13 mm, ε = 1.33 % and P ≈ 3.7 N, the same click as PLA. At 12 mm, ε = 1.56 % and P ≈ 4.7 N. Both stay below 2 %. Fillet the root with r ≈ 0.5 t = 0.75 mm.

Third reading: time. If the clip stays deflected while closed, its force drains away through relaxation. Design it to rest unloaded when engaged: the hook drops behind the edge and the arm springs back straight. The retention angle and the undercut follow the rules in Print-friendly snap fits.

Moduli and strains for printed parts are starting estimates. Confirm them with the cycle test in Testing a mechanism before you trust it.

Plastics that deserve a line of their own

PP. Print it at 220–250 °C onto a PP sheet or packing tape, because it barely sticks to anything else. It shrinks 1.5–2.5 %, so fits drift and large flat parts warp. It is the only near-rigid plastic that works for living hinges. Never trust it with load: its glass transition is below zero and it creeps at room temperature. Its grades and moduli are compared in Polypropylene.

PA and PA-CF. Unfilled nylon, once conditioned, is the toughest choice for clips and sliding parts, but it absorbs water. Dry it before printing (80–85 °C for 8–12 h) and expect it to soften and swell slightly in use. PA-CF or PA-GF is stiff, creeps little along the bead and works very well for gears, brackets and insert bosses. Its elongation is low: never use it for a clip that flexes repeatedly or for a flexure. It needs a hardened nozzle. The rest is in Nylons and polyamides and Carbon and glass fiber filaments.

POM (acetal). This is the plastic of molded industrial gears, bushings and racks: low friction and good fatigue life. It can be printed, but as of late 2026 it is still a specialist filament. It hardly sticks to any standard bed (it needs a specific adhesive, tape or a dedicated sheet), shrinks more than ABS and wants an enclosed printer. Manufacturers do not even agree on the bed temperature. Use it for a gear or bushing you cannot buy, not as a default.

Low-friction filaments. Also called tribological filaments, these are made for printed bushings, nuts and gears that slide on steel; igus's iglidur range is one example. Some grades need an enclosed printer, but the entry grade (i150-type) prints on an open machine. As a starting point, assume a coefficient of friction of 0.1–0.2 dry on steel; wear is covered in Friction and wear.

Fiber-filled filaments in general. They are the stiffest and creep the least along the bead. Between layers, design with 30 % of their XY strength. They also take less strain than PLA before breaking. Use them for brackets, levers, gears and housings, and for nothing that clicks or flexes.

TPU. For soft springs, seals, wheels and grips; never for carrying load. Use 95A when the part must hold its shape and 85A when it must be soft. Hardness and how to print it are in TPU and flexible filaments.

"Tough" PLA (PLA+, Tough). There is no standard behind the name. It is usually softer than basic PLA, because it carries impact modifiers, and then it creeps more. It will not save a clip that snaps: for that, change material family.

Switching material without losing your fits

A new material prints to different dimensions. Shrinkage runs from 0.2–0.5 % for PLA to 0.5–0.8 % for ABS and PC, 1–2 % for PA and 1.5–2.5 % for PP, but on a small part that matters little: what really moves the fit is how each material extrudes and settles, and its surface finish. PA also grows as it takes up water. Repeat the clearance coupon for each material: Real printed clearances and Test coupons. The difference between running and locating clearance is explained in Clearances for moving parts.

Resize the flexing parts too. A clip sized to PLA's 1 % has strain margin to spare in PETG: safe, but softer. One sized to PP's 6 % snaps in PLA on the first opening. The rule: when you move to a material that takes less strain, lengthen the arm by √(ε_old / ε_new). From PETG to PLA, the 10.6 mm arm becomes 15 mm.

When it fails

Material choice failures
Symptom Cause Fix
The PLA clip cracks at the root after a few hundred openings amplitude above 1 % in a brittle plastic lengthen the arm to ε ≤ 1 % or move to PETG, PC or PA; fillet r ≈ 0.5 t
The same file in PETG gives a weak click and the lid rattles modulus 36 % lower shorten the arm and check ε ≤ 2 %, or thicken t (force goes with t³, strain with t: check ε ≤ 2 % again)
The latch or clamp loses grip within weeks relaxation of a part that spends its time deflected make it rest unloaded; or PC, ASA, fiber-filled filament; or a steel spring
Works in winter, but in summer or in the car it goes slack or distorts service temperature above HDT − 15–20 °C ASA or PC unloaded; loaded in the sun, PA-CF, PET-CF or PPA-CF
The PETG or PLA living hinge cracks in fewer than a thousand folds, often far fewer wrong material for large repeated folds PP or TPU, beads perpendicular to the fold
The pin or guide squeaks, binds or wears oval the same soft plastic against itself different materials: PA, POM or low-friction filament, or a steel pin
The carbon-fiber clip snaps on the first try takes less strain than PLA unfilled PETG, PC or PA for anything that bends
The nylon part goes loose or swollen after a few days absorbs moisture, softens and grows dry it before printing and set dimensions once conditioned; or move to PA-CF or PETG

How to test it

Print the same clip in both candidate materials and open and close them until they break or reach 1000 openings. A preloaded part passes only after the 48-hour test: readings at 1 h, 24 h and 48 h, extended on a logarithmic time scale (Testing a mechanism before you trust it). Run it at the part's working temperature; if the extrapolated loss exceeds what the mechanism tolerates, move one step up the creep ranking or redesign so the part rests unloaded.

See also

Design it in KapyCAD

Model the joint with these dimensions. Each one stays a value you can change after the first test print.

Free plan, no card. Runs in your browser, nothing to install.

Open the editor

Still have a question?